PTT PUBLIC COMPANY LIMITED RATCHABURI WORLD COGENERATION COMPANY LIMITED
GAS PIPELINE AND GAS METERING AND REGULATING STATION PROJECT
DOCUMENT TITLE: WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS)
DOCUMENT NO.: PR-W-1102.21-4012-001 REVISION: 0
0 02/04/13 Issued for Construction WS JR NP
A 29/01/13 Issued for Approval WS JR NP
Rev. Date DescriptionPrepared
ByChecked
ByApproved
By
CONTRACTOR:
SIAM RAJATHANEE JOINT VENTURE
CONSULTANT:
UNITY ENGINEERING AND CONSULTANCY
SERVICES CO.,LTD.
REVIEW STAMP COMMENTS
E. Work may proceed.
F. Work may proceed. Submit “for Construction”
Documents.
G. Revise and Resubmit. Work may proceed Subject to incorporation of changes indicated.
H. Revise and Resubmit. Work may not proceed.
I. Review not required. Work may proceed.
Acceptance in any of these categories shall be in no way relieve the Contractor/Supplier of its responsibility for the due and proper performance of the Work in accordance with the Contract/Purchase Order.
Name:
Sign:
Date:
![Page 2: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/2.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING AND REGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 2 of 45
DOCUMENT CHANGE RECORD
Rev Date Prepared/
Revised
By
Reviewed By
Approved By
Description
A 29/01/13 WS JR NP Issued for Approval
0 02/04/13 WS JR NP Issued for Construction
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 3: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/3.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 3 of 20
TABLE OF CONTENT
ARTICLE PAGE
1.0 General.................................................................................................................................................. 4
2.0 Scope of Work....................................................................................................................................... 4
3.0 Reference.............................................................................................................................................. 4
4.0 List of Welding Procedure Specification: (WPS)....................................................................................4
4.1 WPS No. API/D-2.375/T-0.188/Y-42.....................................................................................................5
4.2 WPS No. API/2.375-D-12.75/T-0.188/Y-42...........................................................................................6
4.3 WPS No. API/2.375-D-12.75/0.188-T-0.75/Y-42...................................................................................7
4.4 WPS No. API/12.75-D/0.188-T-0.75/Y-42.............................................................................................8
4.5 WPS No. API/12.75-D/0.188-T-0.75/42-Y-65........................................................................................9
4.6 WPS No. API/12.75-D/0.188-T-0.75/65-Y...........................................................................................10
4.7 WPS No. API/12.75-D/0.75-T/65-Y.....................................................................................................11
5.0 WPS for Weld Repair........................................................................................................................... 12
5.1 WPS No. 1st and 2nd Repair API/D-2.375/T-0.188/Y-42.......................................................................13
5.2 WPS No. 1st and 2nd Repair API/2.375-D-12.75/T-0.188/Y-42.............................................................14
5.3 WPS No. 1st and 2nd Repair API/2.375-D-12-75/0.188-T-0.75/Y-42.....................................................15
5.4 WPS No. 1st and 2nd Repair API/12.75-D/0.188-T-0.75/Y-42...............................................................16
5.5 WPS No. 1st and 2nd Repair API/12.75-D/0.188-T-0.75/42-Y-65..........................................................17
5.6 WPS No. 1st and 2nd Repair API/12.75-D/0.188-T-0.75/65-Y...............................................................18
5.7 WPS No. 1st and 2nd Repair API/12.75-D/0.75-T/65-Y.........................................................................19
ATTACHMENT................................................................................................................................................. 20
PTT Welding Procedure Specification (SP-W-000-01 Rev.0)................................................................20
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 4: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/4.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 4 of 20
1.0 General
This Welding Procedure Specification had been duplicated from PTT welding procedure specification which established and qualified by PTT PLC. And proposed for construction, maintenance, modification and repairing all of PTT gas pipeline and station.
2.0 Scope of Work
This welding procedure specification is proposed for all welding work of Gas Pipeline And Gas Metering and Regulating Station Project if essential variables as describes in API 1104 are not changed then this procedure should applied without the need for requalification.
3.0 Reference
API 1104 standard for welding of pipelines and related facilitiesSP-W-000-07 Rev.0 PTT Welding Procedure Specification (WPS)SP-W-1102.21-010-003 Onshore Pipeline Automatic and Manual Welding
4.0 List of Welding Procedure Specification: (WPS)
Item WPS No.Range Application
OD (in) T (in) SMYS (psi)
4.1 API/D-2.375/T-0.188/Y-42 OD<2.375 T<0.188 SMYS≤42,000
4.2 API/2.375-D-12.75/T-0.188/Y-42 2.375≤OD≤12.75 T<0.188 SMYS≤42,000
4.3 API/2.375-D-12.75/0.188-T-0.75/Y-42 2.375≤OD≤12.75 0.188≤T≤0.75 SMYS≤42,000
4.4 API/12.75-D/0.188-T-0.75/Y-42 OD≤12.75 0.188≤T≤0.75 SMYS≤42,000
4.5 API/12.75-D/0.188-T-0.75/42-Y-65 OD≤12.75 0.188≤T≤0.75 42,000<SMYS<65,000
4.6 API/12.75-D/0.188-T-0.75/65-Y OD≤12.75 0.188≤T≤0.75 SMYS≥65,000
4.7 API/12.75-D/0.75-T/65-Y OD≤12.75 T>0.75 SMYS≥65,000
Note The Welding electrodes “KOBE” brand are proposed
OD mean Outside diameter pipe
T mean Pipe wall thickness
SMYS mean Specific minimum yield strength
WPS mean Welding Procedure Specification
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 5: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/5.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 5 of 20
4.1 WPS No. API/D-2.375/T-0.188/Y-42
PROCEDURE SPECIFICATION NO. API/D-2.375/T-0.188/Y-42
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING AND REGULATING STATION PROJECT Pipe and fittings
Process GTAWMaterial API 5L, SMYS ≤ 42,000 Pipe outside diameter and wall thickness DIA < 2.375”, THICKNESS < 0.188”Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6Electrical or flame characteristics DC-Position FIX 5GDirection of welding VERT.UPNo. of welder 1Tim lapse between passes 180s maxType and removal of lineup clamp EXTERNAL LINEUP CLAMP,REMOVE AFTER 50% ROOT COMPLETE Cleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYPreheat/stress relief n/aShielding gas and flow rate Ar. 20 lpmShielding flux n/aSpeed of travel 3-6 in/minPlasma gas flow rate n/aPlasma gas composition n/aPlasma gas orifice size n/aSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1 ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2 and 3 ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 6: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/6.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 6 of 20
4.2 WPS No. API/2.375-D-12.75/T-0.188/Y-42
PROCEDURE SPECIFICATION NO. API/2.375-D-12.75/T-0.188/Y-42
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING AND REGULATING STATION PROJECT Pipe and fittings
Process GTAWMaterial API 5L, SMYS ≤ 42,000 Pipe outside diameter and wall thickness 2.375”≤ DIA ≤ 12.75”, THICKNESS < 0.188”Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6Electrical or flame characteristics DC-Position FIX 5GDirection of welding VERT.UPNo. of welder 1 or 2Tim lapse between passes 180s maxType and removal of lineup clamp EXTERNAL LINEUP CLAMP,REMOVE AFTER 50% ROOT COMPLETE Cleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYPreheat/stress relief n/aShielding gas and flow rate Ar. 20 lpmShielding flux n/aSpeed of travel 3-6 in/minPlasma gas flow rate n/aPlasma gas composition n/aPlasma gas orifice size n/aSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1 ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2 and 3 ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 7: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/7.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 7 of 20
4.3 WPS No. API/2.375-D-12.75/0.188-T-0.75/Y-42
PROCEDURE SPECIFICATION NO. API/2.375-D-12.75/0.188-T-0.75/Y-42
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING AND REGULATING STATION PROJECT Pipe and fittings
Process GTAW and SMAWMaterial API 5L, SMYS ≤ 42,000 Pipe outside diameter and wall thickness 2.375”≤ DIA ≤ 12.75”, 0.188” ≤ THICKNESS < 0.75”Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6 (2 Beads) E7016 (n Beads)Electrical or flame characteristics DC- DC+Position FIX 5G FIX 5GDirection of welding VERT.UP VERT.UPNo. of welder 1 or 2 1 or 2Tim lapse between passes 180s max 180s maxType and removal of lineup clamp EXTERNAL LINEUP CLAMP,REMOVE AFTER 50% ROOT COMPLETE Cleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYPreheat/stress relief n/aShielding gas and flow rate Ar. 20 lpm n/aShielding flux n/a as electrodeSpeed of travel 3-6 in/min 2-6 in/minPlasma gas flow rate n/aPlasma gas composition n/aPlasma gas orifice size n/aSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1(GTAW) ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2(GTAW) ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm3(SMAW) E7016(4.0 mm) 20-24 90-140 (DCEP) 2-5 ipm
4 to…n(SMAW) E7016(3.2 mm) 20-24 90-120 (DCEP) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 8: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/8.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 8 of 20
4.4 WPS No. API/12.75-D/0.188-T-0.75/Y-42
PROCEDURE SPECIFICATION NO. API/12.75-D/0.188-T-0.75/Y-42
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING AND REGULATING STATION PROJECT Pipe and fittings
Process GTAW and SMAWMaterial API 5L, SMYS ≤ 42,000 Pipe outside diameter and wall thickness 12.75”< DIA , 0.188” ≤ THICKNESS ≤ 0.75”Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6 (2 Beads) E7016 (n Beads)Electrical or flame characteristics DC- DC+Position FIX 5G FIX 5GDirection of welding VERT.UP VERT.UPNo. of welder 1 or 2 1 or 2Tim lapse between passes 180s max 180s maxType and removal of lineup clamp EXTERNAL LINEUP CLAMP,REMOVE AFTER 50% ROOT COMPLETE Cleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYPreheat/stress relief n/aShielding gas and flow rate Ar. 20 lpm n/aShielding flux n/a as electrodeSpeed of travel 3-6 in/min 2-6 in/minPlasma gas flow rate n/aPlasma gas composition n/aPlasma gas orifice size n/aSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1(GTAW) ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2(GTAW) ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm3(SMAW) E7016(4.0 mm) 20-24 90-140 (DCEP) 2-5 ipm
4 to…n(SMAW) E7016(3.2 mm) 20-24 90-120 (DCEP) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 9: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/9.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 9 of 20
4.5 WPS No. API/12.75-D/0.188-T-0.75/42-Y-65
PROCEDURE SPECIFICATION NO. API/12.75-D/0.188-T-0.75/42-Y-65
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING AND REGULATING STATION PROJECT Pipe and fittings
Process GTAW and SMAWMaterial API 5L, 42,000 ≤ SMYS ≤ 65,000Pipe outside diameter and wall thickness 12.75” ≤ DIA , 0.188” ≤ THICKNESS ≤ 0.75”Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6 (2 Beads) E7016 (n Beads)Electrical or flame characteristics DC- DC+Position FIX 5G FIX 5GDirection of welding VERT.UP VERT.UPNo. of welder 1 or 2 1 or 2Tim lapse between passes 180s max 180s maxType and removal of lineup clamp EXTERNAL LINEUP CLAMP,REMOVE AFTER 50% ROOT COMPLETE Cleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYPreheat/stress relief n/aShielding gas and flow rate Ar. 20 lpm n/aShielding flux n/a as electrodeSpeed of travel 3-6 in/min 2-6 in/minPlasma gas flow rate n/aPlasma gas composition n/aPlasma gas orifice size n/aSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1(GTAW) ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2(GTAW) ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm3(SMAW) E7016(4.0 mm) 20-24 90-140 (DCEP) 2-5 ipm
4 to…n(SMAW) E7016(3.2 mm) 20-24 90-120 (DCEP) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 10: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/10.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 10 of 20
4.6 WPS No. API/12.75-D/0.188-T-0.75/65-Y
PROCEDURE SPECIFICATION NO. API/12.75-D/0.188-T-0.75/65-Y
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING AND REGULATING STATION PROJECT Pipe and fittings
Process GTAW and SMAWMaterial API 5L 65,000 ≤ SMYSPipe outside diameter and wall thickness 12.75” ≤ DIA , 0.188” ≤ THICKNESS ≤ 0.75”Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6 (2 Beads) E7016 (n Beads)Electrical or flame characteristics DC- DC+Position FIX 5G FIX 5GDirection of welding VERT.UP VERT.UPNo. of welder 1 or 2 1 or 2Tim lapse between passes 180s max 180s maxType and removal of lineup clamp EXTERNAL LINEUP CLAMP,REMOVE AFTER 50% ROOT COMPLETE Cleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYPreheat/stress relief n/aShielding gas and flow rate Ar. 20 lpm n/aShielding flux n/a as electrodeSpeed of travel 3-6 in/min 2-6 in/minPlasma gas flow rate n/aPlasma gas composition n/aPlasma gas orifice size n/aSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1(GTAW) ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2(GTAW) ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm3(SMAW) E7016(4.0 mm) 20-24 90-140 (DCEP) 2-5 ipm
4 to…n(SMAW) E7016(3.2 mm) 20-24 90-120 (DCEP) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 11: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/11.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 11 of 20
4.7 WPS No. API/12.75-D/0.75-T/65-Y
PROCEDURE SPECIFICATION NO. API/12.75-D/0.75-T/65-Y
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING AND REGULATING STATION PROJECT Pipe and fittings
Process GTAW and SMAWMaterial API 5L 65,000 < SMYSPipe outside diameter and wall thickness 12.75” ≤ DIA , 0.75” < THICKNESS Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6 (2 Beads) E7016 (n Beads)Electrical or flame characteristics DC- DC+Position FIX 5G FIX 5GDirection of welding VERT.UP VERT.UPNo. of welder 1 or 2 1 or 2Tim lapse between passes 180s max 180s maxType and removal of lineup clamp EXTERNAL LINEUP CLAMP,REMOVE AFTER 50% ROOT COMPLETE Cleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYPreheat/stress relief n/aShielding gas and flow rate Ar. 20 lpm n/aShielding flux n/a as electrodeSpeed of travel 3-6 in/min 2-6 in/minPlasma gas flow rate n/aPlasma gas composition n/aPlasma gas orifice size n/aSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1(GTAW) ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2(GTAW) ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm3(SMAW) E7016(4.0 mm) 20-24 90-140 (DCEP) 2-5 ipm
4 to…n(SMAW) E7016(3.2 mm) 20-24 90-120 (DCEP) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 12: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/12.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 12 of 20
5.0 WPS for Weld Repair
Item
Repair WPS No.Apply Repair for WPS No.
Item WPS No.
5.1 1st and 2nd Repair API/D-2.375/T-0.188/Y-42 4.1 API/D-2.375/T-0.188/Y-42
5.2 1st and 2nd Repair API/2.375-D-12.75/T-0.188/Y-42 4.2 API/D-2.375-D-12.75/T-0.188/Y-42
5.3 1st and 2nd Repair API/2.375-D-12.75/0.188-T-0.75/Y-42 4.3 API/D-2.375-D-12.75/T-0.188-T-0.75/Y-42
5.4 1st and 2nd Repair API/12.75-D/0.188-T-0.75/Y-42 4.4 API/12.75-D/0.188-T-0.75/Y-42
5.5 1st and 2nd Repair API/12.75-D/0.188-T-0.75/42-Y-65 4.5 API/12.75-D/0.188-T-0.75/42-Y-65
5.6 1st and 2nd Repair API/12.75-D/0.188-T-0.75/65-Y 4.6 API/12.75-D/0.188-T-0.75/65-Y
5.7 1st and 2nd Repair API/12.75-D/0.75-T/65-Y 4.7 API/12.75-D/0.75-T/65-Y
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 13: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/13.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 13 of 20
5.1 WPS No. 1st and 2nd Repair API/D-2.375/T-0.188/Y-42
PROCEDURE SPECIFICATION NO. 1ST and 2nd Repair API/D-2.375/T-0.188/Y-42
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT Pipe and fittings
Process GTAWMaterial API 5L, SMYS ≤ 42,000 (1st Repair Joint)Pipe outside diameter and wall thickness DIA < 2.375”, THICKNESS < 0.188”Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6Electrical or flame characteristics DC-Position FIX 5GDirection of welding VERT.UPNo. of welder 1Tim lapse between passes 180s maxType and removal of lineup clamp n/aCleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYShielding gas and flow rate Ar. 20 lpmShielding flux n/aSpeed of travel 3-6 in/minAdditional for repairingMethod of exploration of the defects From RT, UT or other NDT results or appropriated methodMethod of defect removal Mechanical grinding, Fusion methods are deniedMethod of confirming defect removed All weld removing, PT, MT or other appropriated methodInterpass inspection required Visual InspectionSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1 ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2 and 3 ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 14: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/14.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 14 of 20
5.2 WPS No. 1st and 2nd Repair API/2.375-D-12.75/T-0.188/Y-42
PROCEDURE SPECIFICATION NO. 1st and 2nd Repair API/2.375-D-12.75/T-0.188/Y-42
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT Pipe and fittings
Process GTAWMaterial API 5L, SMYS ≤ 42,000 Pipe outside diameter and wall thickness 2.375” ≤ DIA ≤ 12.75”, THICKNESS < 0.188”Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6 (2 Beads)Electrical or flame characteristics DC-Position FIX 5GDirection of welding VERT.UPNo. of welder 1Tim lapse between passes 180s maxType and removal of lineup clamp n/aCleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYShielding gas and flow rate Ar. 20 lpmShielding flux n/aSpeed of travel 3-6 in/minAdditional for repairingMethod of exploration of the defects From RT, UT or other NDT results or appropriated methodMethod of defect removal Mechanical grinding, Fusion methods are deniedMethod of confirming defect removed All weld removing, PT, MT or other appropriated methodInterpass inspection required Visual InspectionSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1 ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2 and 3 ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 15: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/15.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 15 of 20
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 16: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/16.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 16 of 20
5.3 WPS No. 1st and 2nd Repair API/2.375-D-12-75/0.188-T-0.75/Y-42
PROCEDURE SPECIFICATION NO. 1st and 2nd Repair API/2.375-D-12-75/0.188-T-0.75/Y-42
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT Pipe and fittings
Process GTAW and SMAWMaterial API 5L, SMYS ≤ 42,000 Pipe outside diameter and wall thickness 2.375” ≤ DIA ≤ 12.75”, 0.188” ≤ THICKNESS ≤ 0.75”Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6 (2 Beads) E7016 (n Beads)Electrical or flame characteristics DC- DC+Position FIX 5G FIX 5GDirection of welding VERT.UP VERT.UPNo. of welder 1 or 2 1 or 2Tim lapse between passes 180s max 180s maxType and removal of lineup clamp n/a n/aCleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYShielding gas and flow rate Ar. 20 lpm n/aShielding flux n/a as electrodeSpeed of travel 3-6 in/min 2-6 in/minAdditional for repairingMethod of exploration of the defects From RT, UT or other NDT results or appropriated methodMethod of defect removal Mechanical grinding, Fusion methods are deniedMethod of confirming defect removed All weld removing, PT, MT or other appropriated methodInterpass inspection required Visual InspectionSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1(GTAW) ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2(GTAW) ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm3(SMAW) E7016 (4.0 mm) 20-24 90-140 (DCEP) 2-5 ipm
4 to…n (SMAW) E7016 (3.2 mm) 20-24 90-120 (DCEP) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 17: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/17.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 17 of 20
5.4 WPS No. 1st and 2nd Repair API/12.75-D/0.188-T-0.75/Y-42
PROCEDURE SPECIFICATION NO. 1st and 2nd Repair API/12.75-D/0.188-T-0.75/Y-42
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT Pipe and fittings
Process GTAW and SMAWMaterial API 5L, SMYS ≤ 42,000 Pipe outside diameter and wall thickness 12.75” < DIA, 0.188” ≤ THICKNESS ≤ 0.75”Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6 (2 Beads) E7016 (n Beads)Electrical or flame characteristics DC- DC+Position FIX 5G FIX 5GDirection of welding VERT.UP VERT.UPNo. of welder 1 or 2 1 or 2Tim lapse between passes 180s max 180s maxType and removal of lineup clamp n/a n/aCleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYShielding gas and flow rate Ar. 20 lpm n/aShielding flux n/a as electrodeSpeed of travel 3-6 in/min 2-6 in/minAdditional for repairingMethod of exploration of the defects From RT, UT or other NDT results or appropriated methodMethod of defect removal Mechanical grinding, Fusion methods are deniedMethod of confirming defect removed All weld removing, PT, MT or other appropriated methodInterpass inspection required Visual InspectionSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1(GTAW) ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2(GTAW) ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm3(SMAW) E7016 (4.0 mm) 20-24 90-140 (DCEP) 2-5 ipm
4 to…n (SMAW) E7016 (3.2 mm) 20-24 90-120 (DCEP) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 18: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/18.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 18 of 20
5.5 WPS No. 1st and 2nd Repair API/12.75-D/0.188-T-0.75/42-Y-65
PROCEDURE SPECIFICATION NO. 1st and 2nd Repair API/12.75-D/0.188-T-0.75/42-Y-65
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT Pipe and fittings
Process GTAW and SMAWMaterial API 5L, 42,000 ≤ SMYS ≤ 65,000 Pipe outside diameter and wall thickness 12.75” ≤ DIA, 0.188” ≤ THICKNESS ≤ 0.75”Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6 (2 Beads) E7016 (n Beads)Electrical or flame characteristics DC- DC+Position FIX 5G FIX 5GDirection of welding VERT.UP VERT.UPNo. of welder 1 or 2 1 or 2Tim lapse between passes 180s max 180s maxType and removal of lineup clamp n/a n/aCleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYShielding gas and flow rate Ar. 20 lpm n/aShielding flux n/a as electrodeSpeed of travel 3-6 in/min 2-6 in/minAdditional for repairingMethod of exploration of the defects From RT, UT or other NDT results or appropriated methodMethod of defect removal Mechanical grinding, Fusion methods are deniedMethod of confirming defect removed All weld removing, PT, MT or other appropriated methodInterpass inspection required Visual InspectionSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1(GTAW) ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2(GTAW) ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm3(SMAW) E7016 (4.0 mm) 20-24 90-140 (DCEP) 2-5 ipm
4 to…n (SMAW) E7016 (3.2 mm) 20-24 90-120 (DCEP) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 19: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/19.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 19 of 20
5.6 WPS No. 1st and 2nd Repair API/12.75-D/0.188-T-0.75/65-Y
PROCEDURE SPECIFICATION NO. 1st and 2nd Repair API/12.75-D/0.188-T-0.75/65-Y
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT Pipe and fittings
Process GTAW and SMAWMaterial API 5L, 65,000 < SMYSPipe outside diameter and wall thickness 12.75” ≤ DIA, 0.188” ≤ THICKNESS ≤ 0.75”Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6 (2 Beads) E7016 (n Beads)Electrical or flame characteristics DC- DC+Position FIX 5G FIX 5GDirection of welding VERT.UP VERT.UPNo. of welder 1 or 2 1 or 2Tim lapse between passes 180s max 180s maxType and removal of lineup clamp n/a n/aCleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYShielding gas and flow rate Ar. 20 lpm n/aShielding flux n/a as electrodeSpeed of travel 3-6 in/min 2-6 in/minAdditional for repairingMethod of exploration of the defects From RT, UT or other NDT results or appropriated methodMethod of defect removal Mechanical grinding, Fusion methods are deniedMethod of confirming defect removed All weld removing, PT, MT or other appropriated methodInterpass inspection required Visual InspectionSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1(GTAW) ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2(GTAW) ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm3(SMAW) E7016 (4.0 mm) 20-24 90-140 (DCEP) 2-5 ipm
4 to…n (SMAW) E7016 (3.2 mm) 20-24 90-120 (DCEP) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 20: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/20.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 20 of 20
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 21: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/21.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 21 of 20
5.7 WPS No. 1st and 2nd Repair API/12.75-D/0.75-T/65-Y
PROCEDURE SPECIFICATION NO. 1st and 2nd Repair API/12.75-D/0.75-T/65-Y
For PIPING/PIPELINE CONSTRUCTION SERVICES Welding of GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT Pipe and fittings
Process GTAW and SMAWMaterial API 5L, 65,000 < SMYSPipe outside diameter and wall thickness 12.75” ≤DIA, 0.75” <THICKNESS Joint design BUTT JOINT 75 degree “SINGLE VEE”Filler metal and no. of beads ER70S-6 (2 Beads) E7016 (n Beads)Electrical or flame characteristics DC- DC+Position FIX 5G FIX 5GDirection of welding VERT.UP VERT.UPNo. of welder 1 or 2 1 or 2Tim lapse between passes 180s max 180s maxType and removal of lineup clamp n/a n/aCleaning and/or grinding SLAG REMOVE BY HAMMERING, BRUSHING THEN GRINDING IF NECESSARYShielding gas and flow rate Ar. 20 lpm n/aShielding flux n/a as electrodeSpeed of travel 3-6 in/min 2-6 in/minAdditional for repairingMethod of exploration of the defects From RT, UT or other NDT results or appropriated methodMethod of defect removal Mechanical grinding, Fusion methods are deniedMethod of confirming defect removed All weld removing, PT, MT or other appropriated methodInterpass inspection required Visual InspectionSketches and tabulations attached as below
ELECTRODE SIZE AND NUMBER OF BEADSLayer Number Electrode Size and Type Voltage Amperage and Polarity Speed
1(GTAW) ER70S-6 (2.4 mm) 18-24 100-150 (DCEN) 3-6 ipm2(GTAW) ER70S-6 (2.4 mm) 18-24 120-200 (DCEN) 3-6 ipm3(SMAW) E7016 (4.0 mm) 20-24 90-140 (DCEP) 2-5 ipm
4 to…n (SMAW) E7016 (3.2 mm) 20-24 90-120 (DCEP) 3-6 ipm
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 22: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/22.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 22 of 20
ATTACHMENT
PTT Welding Procedure Specification (SP-W-000-01 Rev.0)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 23: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/23.jpg)
WELDING PROCEDURE SPECIFICATION FOR PIPING AND
PIPELINE (WPS)
GAS PIPELINE AND GAS METERING ANDREGULATING STATION PROJECT
Document No. PR-W-1102.21-4012-001
Rev. 0 Page 23 of 20
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 24: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/24.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 25: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/25.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 26: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/26.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 27: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/27.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 28: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/28.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 29: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/29.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 30: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/30.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 31: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/31.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 32: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/32.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 33: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/33.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 34: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/34.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 35: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/35.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 36: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/36.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 37: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/37.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 38: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/38.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 39: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/39.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 40: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/40.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 41: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/41.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 42: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/42.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 43: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/43.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 44: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/44.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))
![Page 45: Pr-w-1102.21-4012-001 Rev 0 Welding Procedure Specification for Piping and Pipeline (Wps)-Sw(1)](https://reader033.vdocuments.us/reader033/viewer/2022061607/55cf99bc550346d0339eea54/html5/thumbnails/45.jpg)
PR-W-1102.21-4012-001 Rev.0(WELDING PROCEDURE SPECIFICATION FOR PIPING AND PIPELINE (WPS))