welding procedure_plate hook.docx
TRANSCRIPT
![Page 1: Welding procedure_plate hook.docx](https://reader036.vdocuments.us/reader036/viewer/2022083007/563dbade550346aa9aa8b71d/html5/thumbnails/1.jpg)
WELDING PROCEDURE FOR PLATEHOOK
1. Positioning of the Handle: Handle to be positioned on desired location. Positioning should be done taken into account the possibility of obstruction of the handle during the lifting operation.
2. Welding Seam preparation: Weld seams are to be clean. It has to be checked that they are free from paint, grease, oil,..
3. Weather Protection, Preheating: -Weld seams are to be sufficiently protected against climatic influences (wind, damp, rain,..)-Preheating of the material till 110°C is required. Interpass temperature should be well above this. T 8/5 time should be between 5s and 20s.
4. Welding: -Fillet weld with throat thickness 3mm all around the handle.
-Electrodes to be used: AWS.60xx, 70xx or equivalent.
WELDING INSTRUCTIONS FOR PLATEHOOK www.contech.be