institut za varilstvo g instit ute - bimontbimont.si/en/certificates_files/wic.pdf · welding...

6
USNAS Reg. No. 256/1-028 INSTITUT ZA VARILSTVO Weld i n g Instit ute Institutzavarilstvod.o.o.,Ptujska19,SI-1000Ljubljana Sheet lil INSPECTION BODY - WELDING PROCEDURES Welding procedure approval (WPAR) in accordance with 51ST EN ISO 15614-1 + GL2000 No.: 33922/11 (E) Ljubljana, 09 Sept., 2011 Client 1 BIMONT d.o.o., Senčna ulica 19, 6310 Izola Date of welding 1 Sveti Anton, 12 July, 2011 I DN: 1_6_8_98 _ The test pieces were produced on steel mat. no: W.Nr.:1.0570 (S355J2+N) and fulfil following' requirements: Tensile test Rmin ranqe 490-630 N/mmL Hardness HV10: <380HV Bend angle 180° Imperfect shape - permitted for quality level C in accordance with EN ISO 5817 Impacttoughnes: <':27JpriT= -20°C Internal imperfections - permitted for quality level B in accordance with EN ISO 5817 Range of approval: Weldinq process MAG (136) Type ofweld Butt weld BW ss Material and group (SIST-TP CEN ISOfTR 15608) steel with nominal elastic limit Re:5355 N/mm2 (gruppe1.1, 1.2) Thickness (mm) from 3,0 to 24,0 Outer diameter (mm) above 0500,0 Filler material EN ISO 17632-A: T 46 4 C/M1 H5 Type of current DC (+) Welding position PF Welding process Shielding gas: CO 2 (in acc. to SIST EN ISO 14175: C1) Shieldinq root: ceramic backinq I The approval of the welding procedure is based on the test results stated in Report no.: 33922/11 (E). It is certified herewith that the test welds were prepared, welded and tested in accordance with the requirements of the test specifications and standards indicated above. ""$" .1 -' .,;r-' ;;"il'" ~ ,.,,.<. ~ •.. Thedocumentmaybecopiesonlyasawhole! Obr.: OP-s; rev. 11, Priloga 3

Upload: others

Post on 24-Mar-2020

4 views

Category:

Documents


0 download

TRANSCRIPT

Page 1: INSTITUT ZA VARILSTVO g Instit ute - BIMONTbimont.si/en/Certificates_files/WIC.pdf · Welding procedure approval (WPAR) in accordance with 51ST EN ISO 15614-1 + GL2000 No: 33923/11

USNASReg. No. 256/1-028

INSTITUT ZA VARILSTVOWel d in g I n s tit ute

Institutzavarilstvod.o.o.,Ptujska19,SI-1000Ljubljana Sheet lil

INSPECTION BODY - WELDING PROCEDURES

Welding procedure approval (WPAR) in accordance with 51ST EN ISO15614-1 + GL2000

No.: 33922/11 (E) Ljubljana, 09 Sept., 2011

Client 1 BIMONT d.o.o., Senčna ulica 19, 6310 Izola

Date of welding 1 Sveti Anton, 12 July, 2011 I DN: 1_6_8_98 _

The test pieces were produced on steel mat. no: W.Nr.:1.0570 (S355J2+N) and fulfil following' requirements:Tensile test Rmin ranqe 490-630 N/mmL Hardness HV10: <380HVBend angle 180° Imperfect shape - permitted for quality level C in accordance

with EN ISO 5817Impact toughnes: <':27Jpri T= -20°C Internal imperfections - permitted for quality level B in

accordance with EN ISO 5817

Range of approval:

Weldinq process MAG (136)Type ofweld Butt weld BW ssMaterial and group (SIST-TP CEN ISOfTR 15608) steel with nominal elastic limit Re:5355N/mm2 (gruppe1.1,

1.2)Thickness (mm) from 3,0 to 24,0Outer diameter (mm) above 0500,0Filler material EN ISO 17632-A: T 46 4 C/M1 H5Type of current DC (+)Welding position PFWelding process Shielding gas: CO2 (in acc. to SIST EN ISO 14175: C1)

Shieldinq root: ceramic backinq

I The approval of the welding procedure is based on the test results stated in Report no.: 33922/11 (E).

It is certified herewith that the test welds were prepared, welded and tested in accordance with therequirements of the test specifications and standards indicated above.

""$" .1 -'

.,;r-' ;;"il'"~ ,.,,.<. ~•..

Thedocumentmaybecopiesonlyasawhole!Obr.: OP-s; rev. 11, Priloga 3

Page 2: INSTITUT ZA VARILSTVO g Instit ute - BIMONTbimont.si/en/Certificates_files/WIC.pdf · Welding procedure approval (WPAR) in accordance with 51ST EN ISO 15614-1 + GL2000 No: 33923/11

USNAS

INSTITUT ZA VARILSTVOW el d i n g I n s tit ute

Institut za varilstvo d.o.o., Ptujska 19, SI-1000 Ljubljana

Reg. No. 256/1-028

Sheet lil

INSPECTION BODY - WELDING PROCEDURES

Welding procedure approval (WPAR) in accordance with 51ST EN ISO15614-1 + GL2000

No: 33923/11 (E) Ljubljana, 09 Sept., 2011

Client I BIMONT d.o.o., Senčna ulica 19, 6310 Izola

Date ofwelding I Sveti Anton, 12 July, 2011 ION: 1-=6...:...c89:....:.8 _

The test pieces were produced on steel mat.no.: W.Nr.:1.0570 (S355J2+N) and fulfil following requirementsfor fillet weld:Hardbess HV 10: < 380HV Imperfect shape - permitted for quality level C in accordance

with EN ISO 5817High of weld (mm): <': 6,0 (Muiti pass) Internal imperfections - permitted for quality level B in

accordance with EN ISO 5817

Range of approval:

Welding process MAG (136)Type ofweld Fillet weld FWMaterial and group (SIST-TP CEN ISOlTR 15608) steel with nominal elastic limit Re:5 355 N/mm2 (gruppe.:

1.1, 1.2)Thickness (mm) From 7,5 mm to 14,4 mmOuter diameter (mm) /

Throat thickness (mm) IFiller material EN ISO 17632-A: T 46 4 C/M1 H5Type of current DC (+)Weldinq position PFWelding process Shielding gas: CO2 (in acc. to SIST EN ISO 14175: C1)

I The approval of the welding procedure is based on the test results sta ted in Report no.: 33923/11 (E).

It is certified herewith that the test welds were prepared, welded and tested in accordance with there uirements of the test specifications and standards indicated above.

Slamp:

The document may be copies only as a whole!Obr.: OP-5; rev. 11, Priloga 3

Page 3: INSTITUT ZA VARILSTVO g Instit ute - BIMONTbimont.si/en/Certificates_files/WIC.pdf · Welding procedure approval (WPAR) in accordance with 51ST EN ISO 15614-1 + GL2000 No: 33923/11

VSNASReg. No. 256/1-028

INSTITUT ZA VARILSTVOW el d in g I n s tit ute

Institutzavarilstvod.o.o.,Ptujska19,SI-1000Ljubljana Sheet 111

INSPECTION BODY - WELDING PROCEDURES

Welding procedure approval (WPAR) in accordance with 51ST EN ISO15614-1 + GL2000

33924/11 (E)No: Ljubljana, 09 Sept., 2011

Client I BIMONT d.o.o., Senčna ulica 19, 6310 Izola

Date of we Idin9 I Sveti Anton, 14 July, 2011 ION: 16898

The test pieces were produced on steel mat. no: W.Nr.: 1.0570 (S355J2+N) and fulfil foliowinq requirements:Tensile test Rmin range 490-630 Nzmrn" Hardness HV10: <380HVBend angle 180° Imperfect shape - permitted for quality level C in accordance

with EN ISO 5817Impact toughnes: ~27J pri T= -20°C Internal imperfections - permitted for quality level B in

accordance with EN ISO 5817

Range of approval:

Weldinq process E (111)Type ofweld Butt weld BW ss nbMaterial and group (SIST-TP CEN ISOlTR 15608) steel with nominal elastic limit Res355N/mm2 (gruppe1.1,

1.2)Thickness (mm) from 3,0 to 24,0Outer diameter (mm) above 0500,0Filler material EN ISO 2560-A: E 42 4 B 32 H5Tvpe of current De (+)Weldinq position PEWeldinq process /

I The approval of the welding procedure is based on the test results stated in Report no.: 33924/11 (E).

It is certified herewith that the test welds were prepared, welded and tested in accordance with there uirements of the test s ecifications and standards indicated above.

Thedocumentmaybecopiesonlyasawhole!Obr.: DP-5; rev. 11, Priloga 3

Page 4: INSTITUT ZA VARILSTVO g Instit ute - BIMONTbimont.si/en/Certificates_files/WIC.pdf · Welding procedure approval (WPAR) in accordance with 51ST EN ISO 15614-1 + GL2000 No: 33923/11

USNASReg. No. 256/1-028

INSTITUT ZA VARILSTVOW el d i n g I n s tit ute

Institut za varilstvo d.o.o., Ptujska 19, SI-1000 Ljubljana Sheet 111

INSPECTION BODY - WELDING PROCEDURES

Welding procedure approval (WPAR) in accordance with 51ST EN ISO15614-1 + GL2000

33925/11 (E)No: Ljubljana, 09 Sept., 2011

Client I BIMONT d.o.o., Senčna ulica 19, 6310 Izola

Date of welding I Sveti Anton, 14 July, 2011 ION: 1_6_89_8 _

The test pieces were produced on steel mat. no.; W.Nr.:1.0570 (S355J2+N) and fulfil following requirementsfor fillet weld:Hardness HV 10: < 380HV Imperfect shape - permitted for quality level C in accordance

with EN ISO 5817High of weld (mm): ~ 10,0 (Muiti pass) Internal imperfections - permitted for quality level B in

accordance with EN ISO 5817

Range of approval:

Welding process E (111)Type ofweld Fillet weld FWMaterial and group (SIST-TP CEN ISOfTR 15608) steel with nominal elastic limit Re::; 355 N/mm2 (gruppe:

1.1, 1.2)Thickness (mm) From 10,0 mm to 24,0 mmOuter diameter (mm) 1Throat thickness (mm) /Filler material EN ISO 2560-A: E 42 4 B 32 H5Type of current De (+)Welding position POWelding process /

I The approval of the welding procedure is based on the test results stated in Report no.: 33925/11 (E).

It is certified herewith that the test welds were prepared, welded and tested in accordance with there uirements of the test s ecifications and standards indicated above.

The document may be copies only as a whole!Obr.: OP-5; rev. 11, Priloga 3

Page 5: INSTITUT ZA VARILSTVO g Instit ute - BIMONTbimont.si/en/Certificates_files/WIC.pdf · Welding procedure approval (WPAR) in accordance with 51ST EN ISO 15614-1 + GL2000 No: 33923/11

USNASReg. No. 256/1-028

INSTITUT ZA VARILSTVOW el d i n g In s tit ute

Institutzavarilstvod.o.o.,Ptujska19,SI-1000Ljubljana Sheef 111

INSPECTION BODY - WELDING PROCEDURES

Welding procedure approval (WPAR) in accordance with 51ST EN ISO15614-1 + GL2000

33926/11 (E)No.: Ljubljana, 09 Sept., 2011

Client I BIMONT d.o.o., Senčna ulica 19, 6310 Izola

Date of welding I Sveti Anton, 13 July, 2011 ION: 16898

The test pieces were produced on steel mat. no: W.Nr.:1.0570 (S355J2+N) and fulfil followinq requirements:Tensile test Rmin range 490-630 N/mm" Hardness HV10: <380HVBend angle 180° Imperfect shape - permitted for quality level C in accordance

with EN ISO 5817Impact toughnes: ~27J pri T= -20°C Internal imperfections - permitted for quality level B in

accordance with EN ISO 5817

Range of approval:

Weldinq process TIG(141)Type ofweld Butt weld BW ss nbMaterial and group (SIST-TP CEN ISOlTR 15608) steel with nominal elastic limit Re:S355N/mm2 (gruppe1.1,

1.2)Thickness (mm) from 3,0 to 12,6Outer diameter (mm) Above 025,5Filler material EN ISO 14341: G2 MoTvpe of current DG (-)Weldinq position HL045Welding process Shielding gas: Ar (in acc. to SIST EN ISO 14175: 11)

I The approval of the welding procedure is based on the test results stated in Report no.: 33922/11 (E).

It is certified herewith that the test welds were prepared, welded and tested in accordance with there uirements of the test s ecifications and standards indicated above.

Sfamp:

Thedocumentmaybecopiesonlyasawhole!Obr.: DP-5; rev. 11, Priloga 3

Page 6: INSTITUT ZA VARILSTVO g Instit ute - BIMONTbimont.si/en/Certificates_files/WIC.pdf · Welding procedure approval (WPAR) in accordance with 51ST EN ISO 15614-1 + GL2000 No: 33923/11

INSTITUT ZA VARILSTVOW el d in g I n s tit ute

Institut za varilstvo d.o.o., Ptujska 19, SI-1000 Ljubljana

USNASReg. No. 256/1-028

Sheet lil

INSPECTION BODY - WELDING PROCEDURES

Welding procedure approval (WPAR) in accordance with 51ST EN ISO15614-1

No.: 33345/11 (E) Ljubljana, 23 June, 2011

Client 1 BIMONT d.o.o., Senčna ulica 19, 6310 Izola

Date of welding 1 Sveti Anton, 10 June, 2011 ION: 1---'.6--=--85'--'-0 ---'

The test pieces were produced on steel mat.: tube - W.Nr.:1.0345 (P235GH) and plate - W.Nr.: 1.0425(P265GH) and fulfil foliowinq requirements:Hardness HV 10: < 380HV Imperfect shape - permitted for quality level C in accordance

with EN ISO 5817Internal imperfections - permitted for quality level B inaccordance with EN ISO 5817

Range of approval:

Welding process TIG(141)Type ofweld BW T - joint (tube on flanqe)Material and group (SIST-TP CEN ISOfTR 15608) steel with nominal elasticlimit Re:5265N/mm2 (gruppe 1.1)

Thickness (mm) tube: from 3,0 to 7,2 I plate: from 11,0 to 44,0Outer diameter (mm) above 038,0Filier material EN ISO 14341: G2 MoType of current De (-)Welding position PBOther informations Shielding gas: Ar (in ace. to SIST EN ISO 14175: 11)

Obr.: OP-S; rev. 11, Priloga 3

1 The approval of the welding procedure is based on the test results stated in Report no.: 33345/11 (E).

It is certified herewith that the test welds were prepared, welded and tested in accordance with there uirements of the test s ecifieations and standard indieated above.

Head of inspection body:d~J~ZO~1:;