Download - Welding Procedures Specification
-
7/27/2019 Welding Procedures Specification
1/39
Welding Procedure Specification
(WPS)
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
2/39
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
3/39
Preheat Temp.
Range :-
12 mm 30 mm : 20C
31 mm 36 mm : 30C
Heating Method :-
LPG Torch
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
4/39
Interpass Temp.
Maximum : 250C
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
5/39
How to check interpass temp. ?
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
6/39
1. Tempilstik
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
7/39
2. Digital Thermometer
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
8/39
Electrodes
Root E 7016 G
Hot Pass E 7018 1
Filling E 7018 1 Capping E 7018 1
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
9/39
Electrode Brand KobelcoOnly Use this Electrode
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
10/39
Where do you keep electrodes ?
Quiver Oven
What is the temp. of the oven?( 70 C )
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
11/39
Types Of Welding
1. SMAW (Shielded Metal Arc Welding).
2. SAW (Submerged Arc Welding).
3. FCAW (Flux Core Arc Welding).4. GTAW (Gas Tungsten Arc Welding).
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
12/39
SMAW
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
13/39
SAW
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
14/39
FCAW
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
15/39
GTAW
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
16/39
Welding Positions
1G 2G 3G 4G 5G 6G 6GR
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
17/39
1G
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
18/39
2G
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
19/39
3G
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
20/39
4G
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
21/39
5G
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
22/39
6G
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
23/39
6GR
Sara Adel10/6/2013
-
7/27/2019 Welding Procedures Specification
24/39
Welding Defects
What are the defects that we can find in thewelding ?
1. Lack of fusion
2. Lack of penetration
3. Excess penetration4. Concavity or Suck back
5. Porosity
6. Inclusions
7. Cracking
8. Undercut
9. Spatter
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
25/39
1. Lack of fusion
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
26/39
2. Lack of penetration
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
27/39
3. Excess penetration
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
28/39
4. Concavity or Suck back
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
29/39
5. Porosity
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
30/39
6. Inclusions
Examples : Slag
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
31/39
7. Cracking
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
32/39
8. Undercut
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
33/39
9. Spatter
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
34/39
Is this welding good? (Yes/No)
Why?
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
35/39
Perfect Welding
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
36/39
Safety
PPE (Personal Protective Equipment)
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
37/39
1. Follow the WPS
2. Ask your supervisor
3. Try to minimize the using ofGrinder
4. Keep electrodes in the QUIVER Oven
5. Always check (Temp. , Current , Volt ,)
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
38/39
10/6/2013 Sara Adel
-
7/27/2019 Welding Procedures Specification
39/39
10/6/2013 S Ad l