additives primer blown films, cast films & extrusion coatingadditives primer blown films, cast...
TRANSCRIPT
![Page 1: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/1.jpg)
Additives PrimerBlown Films, Cast Films &
Extrusion Coating
Dr. Prakash R. PatelDirector R&DAmpacet Corporation
2007 PLACE Conference
September 16-20
St Louis, MO
![Page 2: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/2.jpg)
“Common” Additives for PE & PP Films
• Slips• Antiblocks• Antistats• Antifogs• Antioxidants• UV absorbers• UV inhibitors• Fillers
![Page 3: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/3.jpg)
“Exotic” Additives
• Nucleating/Clarifying agents• Flame Retardants• Antimicrobials• Oxygen scavengers• Odor absorbers• Desiccants
![Page 4: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/4.jpg)
Processing Temperatures for PE films
• Blown Film- Typically < 400F• Cast Film- Range from 450 to 550F• Extrusion Coating – Generally > 600F• Challenges for high temp. processes
(Cast film & extrusion coating)– Thermal Stability of additives– Moisture adsorption by additives
![Page 5: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/5.jpg)
Slips: Mechanism
Plastic Film
Layers Of Slipmolecules
Slip Migration
Plastic Film
![Page 6: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/6.jpg)
Slips
• Erucamide & Oleamide- most commonly used
• Challenges:– COF Control- Correct Loading– Thermal Stability (CF, EC)– Heat sealing– Printing– Maintenance of corona treatment– Adhesive laminations– Transfer on a roll
![Page 7: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/7.jpg)
Antiblocks- Mechanism
Film with AntiblockFilm without Antiblock
Antiblock Particles PE film layers
![Page 8: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/8.jpg)
Antiblocks
• Diatomaceous earth (DE) and Talc- the most commonly used
• Challenges:– Quality of dispersion– Particle size & film layer ratios– Abrasiveness– Haze/Clarity– Correct loading (Related to polymer type)– Synergy with slips
![Page 9: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/9.jpg)
Antistats- Mechanism Charge Dissipation
Plastic Film
Layer ofAntistatmolecules
Antistat Migration
H HO
H HO
H HO
H HO
![Page 10: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/10.jpg)
Antistats
• Various Chemistries- Amines, Amides & Esters most common
• Challenges:– Knowledge of specifications– Humidity Dependent– Migration slow- properties are time
dependent– Polymer selection (Diff. AS chemistry)– Correct Loading (Multilayer films)
![Page 11: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/11.jpg)
Antistats
• Challenges:– Thermal stability (CF, EC)– Heat Sealing– Printing (Ink Adhesion)– Maintenance of corona treatment– Adhesive Laminations– Other additives
![Page 12: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/12.jpg)
Antifogs- Mechanism
Plastic Film
Layer ofAntifogmolecules
Antifog Migration
Flat film of waterFlat film of water
![Page 13: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/13.jpg)
Antifogs
• Chemistries must be FDA approved– Limited Chemistries
• Challenges:– Migration slow- properties are time
dependent– Polymer selection (Diff. AF chemistry)– Correct Loading (Multilayer films)– Performance dependent on film structure,
type of test, test equipment etc.
![Page 14: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/14.jpg)
Antifogs
• Challenges:– Thermal stability (CF, EC)– Heat Sealing– Printing (Ink Adhesion)– Maintenance of corona treatment– Adhesive Laminations– Other additives
![Page 15: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/15.jpg)
Infrared (IR) : 750 - 35000 nm Visible light : 400 - 750 nm
Red : 647-750 nmOrange : 585-647 nmYellow : 575-585 nmGreen : 490-575 nmBlue : 424-490 nmViolet : 400-424 nm
Ultra Violet (UV) : 200 - 400 nm X Rays : 0.01 - 10 nm
UVUVIRIR
Intensity of the total sun irradiation is expressed in
Kilolangleys (Kly) :
1 Kly = 4.184 KJ/cm2
λ
Electromagnetic Spectrum
![Page 16: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/16.jpg)
UV Absorbers vs. UV Inhibitors
• UV light (high energy)- can degrade the polymer as well as degrade the contents of a plastic package
• UV inhibitors- added to prevent polymer degradation and protect the film or the plastic package itself
• UV absorbers- added to absorb UV light & protect contents of a package– Organic UV absorbers– Inorganic UV absorbers
![Page 17: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/17.jpg)
Efficiency
Lambert-beer’s law
UV absorbency is proportional to additive concentration and filmthicknessOnly for “thick” film (above 100µm)Compatibility limit : 5000-6000ppm
Abs = AbsorbencyAbs = AbsorbencyAbs = k.t.cAbs = k.t.c k = extinction coefficientk = extinction coefficient
t = thicknesst = thicknessc = concentrationc = concentration
Organic UV AbsorbersOrganic UV Absorbers
![Page 18: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/18.jpg)
UV Screening of 100µm films containing 2000ppm Organic UV Absorber 1 (2% 10057) and 2000ppm Organic UV Absorber 2 (100645)
Organic UV AbsorbersOrganic UV Absorbers
200,0 250 300 350 400 450 500 550 600,0-0,1
10
20
30
40
50
60
70
80
91,6
Wavelengths
%T
Pure LDPE
2% 10057
2% 100645
![Page 19: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/19.jpg)
UV Absorbers
• Challenges:– Blocking UV light completely in a thin,
transparent film (< 100 µ)– Organic UVAs
• Additive migration • Yellowish color
– Inorganic UVAs• Quality of dispersion• Haze/poor clarity
![Page 20: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/20.jpg)
UV Inhibitors
• Protect the polymer from degradation caused by exposure to UV light
• Scavenge free radicals• Hindered Amine Light Stabilizers (HALS)
are the most common ones
![Page 21: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/21.jpg)
Auto Oxidation Cycle
R.
ROO.
R.+
ROOH
RO.+HO.
polymer
Oxygen
RH
RHHALS
HALS
HALSUV light/Heat
![Page 22: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/22.jpg)
UV Inhibitors
• Challenges:– Correct loading– Proper selection of HALS– Interaction with other additives– Interaction with acidic chemicals such as
pesticides & herbicides
![Page 23: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/23.jpg)
Antioxidants
• Protect the polymer from thermal degradation– Processing– Long term storage under hot conditions
• Hindered phenols (primary AO) and phosphites (secondary AO) are the most common
![Page 24: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/24.jpg)
Auto Oxidation Cycle
R.
ROO.
R.+
ROOH
RO.+HO.
polymer
Oxygen
RH
RH
Phosphites
Phenols
Phenols
UV light/Heat
![Page 25: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/25.jpg)
Antioxidants
• Challenges:– Discoloration such as pinking or yellowing
caused by phenolic AOs (biggest challenge)
– Hydrolysis of phosphites– Correct loading
![Page 26: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/26.jpg)
SUMMARY
• Additive Challenges:– Proper chemistry selection & correct
loading– Migration (slips, antistats, antifogs)– Thermal Stability/Smoking (cast film &
extrusion coating)– Heat sealing, Printing & Adhesive
Lamination
![Page 27: Additives Primer Blown Films, Cast Films & Extrusion CoatingAdditives Primer Blown Films, Cast Films & Extrusion Coating Dr. Prakash R. Patel Director R&D Ampacet Corporation 2007](https://reader030.vdocuments.us/reader030/viewer/2022011906/5f385708b6bd900d03135321/html5/thumbnails/27.jpg)
Thank You
Prakash R. Patel, Ph.D.Director R&[email protected]
Please remember to turn in your evaluation sheet...