superalloysinfohost.nmt.edu/~ljacobso/superalloy slides.pdf · mete 327 physical metallurgy...
TRANSCRIPT
![Page 1: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/1.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
SUPERALLOYS
METE 327Fall, 2008
![Page 2: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/2.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
OUTLINE Historical perspective Applications Compositions Processes Properties
− Creep
![Page 3: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/3.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 4: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/4.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
Applications Gas Turbine Engines
− Blades, vanes, disks, combustors Space Vehicles
− Rocket motors Nuclear Reactors Submarines Petroleum Equipment
![Page 5: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/5.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 6: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/6.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
Compositions Ni, Co and Fe Based Alloys Solid solution strengthening
− Cr, Mo, Al, Nb, Ti and others Precipitation strengthening
− Mostly due to Al and Ti− Ni3(Al,Ti), gamma prime− Lattice mismatch, amount, size and morphology
Carbide phases− M23C6, M6C or MC− M can be Cr, Ti, Mo or W
![Page 7: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/7.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 8: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/8.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 9: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/9.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 10: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/10.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 11: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/11.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 12: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/12.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 13: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/13.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 14: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/14.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 15: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/15.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 16: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/16.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
Astroloy Microstructure (orig. 15 K X)
![Page 17: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/17.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
CREEP Deformation at high temperature under
constant load Important property of Superalloys Brief discussion now, more next time
![Page 18: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/18.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 19: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/19.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 20: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/20.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 21: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/21.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 22: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/22.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 23: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/23.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
Engineering Design Using Creep (and Stress-Rupture)
The Larson-Miller Parameter:
Stress Rupture Data Plottedaccording to the followingequation:
Where M = log e
and θ = t exp (-Q/RT)
assuming that Q and θ are functions of stress only. t can be atime to rupture or a time to a given creep strain.
Engineering Design Using Creep (and Stress-Rupture)
The Larson-Miller Parameter:
Stress Rupture Data Plottedaccording to the followingequation:
Where M = log e
and θ = t exp (-Q/RT)
assuming that Q and θ are functions of stress only. t can be atime to rupture or a time to a given creep strain.
![Page 24: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/24.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 25: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/25.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 26: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/26.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
Assignment Please email me a question about superalloys
before Monday, 17 November [email protected] More about creep next time, and Materials
Selection for Design
![Page 27: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/27.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08
![Page 28: SUPERALLOYSinfohost.nmt.edu/~ljacobso/Superalloy Slides.pdf · METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson ... time to rupture or a time to a given creep strain](https://reader036.vdocuments.us/reader036/viewer/2022062401/5a72181a7f8b9ab6538d3a4e/html5/thumbnails/28.jpg)
METE 327 Physical Metallurgy Copyright 2008 Loren A. Jacobson 5/16/08