moisture damage and benefits of liquid anti-stripping
TRANSCRIPT
![Page 1: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/1.jpg)
Moisture Damage andBenefits of
Liquid Anti-stripping Additives (LAS)
by
Sundaram Logaraj and James N Anagnos
June 23, 2005
![Page 2: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/2.jpg)
More of a problem in recent years
Moisture Damage or Strippingin Asphalt Pavements
![Page 3: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/3.jpg)
Moisture Damage SurveyGary Hicks -1985
34 States…..yes
12 States…..no
4 States…..no response
![Page 4: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/4.jpg)
Survey – Gary Hicks &Tim Aschenbrener* – 08/2002
Problem Hicks 1985
Aschenbrener 2002
Yes 34 44
No or Rarely 12 9
No Response 4
*Colorado DOT
![Page 5: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/5.jpg)
Tim Aschenbrenner Survey, CODOT - 2002
Treatment
Lime Lime or liquidsLiquidsLiquids seldomNo or rarely
![Page 6: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/6.jpg)
Factors to Minimize Moisture Damage*
1. Good Mix Design- Specifications- Aggregates- Testing for moisture damage
and suitable treatment
Moisture Sensitivity Subcommittee,Asphalt Institute 2002
![Page 7: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/7.jpg)
Factors to Minimize Moisture Damage*
2. Field and Construction Practices– Avoid stockpile segregation– Proper drying of aggregate– Proper compaction to required densities
– Adequate pavement drainage
Moisture Sensitivity Subcommittee,Asphalt Institute 2002
![Page 8: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/8.jpg)
Premature Failure of Asphalt Overlays From Stripping:
Case Histories
ByPrithvi S. Kandhal
Ian Rickards
![Page 9: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/9.jpg)
Pennsylvania Turnpike (Cumberland County)
• Work performed (Nov. 1994)– existing pavement milled to 40 mm depth– replaced with 9.5 mm size dense HMA
• Premature distress observed (early 1995)• Pavement inspected (July 1996)
![Page 10: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/10.jpg)
![Page 11: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/11.jpg)
![Page 12: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/12.jpg)
![Page 13: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/13.jpg)
Interstate 40 in Oklahoma
• Work performed (October 1990)– 90 mm cold milling– placed 70 mm thick Type “F” mix (25 mm
top size) in both EB and WB lanes
![Page 14: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/14.jpg)
Interstate 40 in Oklahoma
– placed 19 mm thick OGFC in EB lanes– placed 25 mm thick dense “E” mix in WB
lanes because “F” mix was taking in water• Potholing observed in EB lanes• Pavement inspected in September 1991
![Page 15: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/15.jpg)
![Page 16: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/16.jpg)
![Page 17: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/17.jpg)
![Page 18: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/18.jpg)
Will Rogers Pkwy in Oklahoma
• Work performed (June 1992)– mill existing 20 mm thick OGFC– replace with 25 mm thick dense
HMA (Type B)
![Page 19: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/19.jpg)
Will Rogers Pkwy in Oklahoma
• Potholing observed in July 1992• Inspected in July 1992
![Page 20: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/20.jpg)
![Page 21: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/21.jpg)
![Page 22: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/22.jpg)
![Page 23: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/23.jpg)
![Page 24: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/24.jpg)
Hume Highway in NSW, Australia
• Overlay work performed (June 1993)– 80 mm thick dense HMA (25 mm mix)– 35 mm thick dense HMA (12.5 mm
mix)–30 mm thick OGFC
![Page 25: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/25.jpg)
Hume Highway in NSW, Australia
• Potholing observed in SB lanes (February 1995)
• No potholing in NB lanes (?)
![Page 26: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/26.jpg)
![Page 27: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/27.jpg)
![Page 28: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/28.jpg)
Adhesion and Stripping
• What are Adhesion and Stripping• Contributing factors• What are Anti-stripping Additives• How do they prevent stripping• Adhesion Vs Cohesion• What is being measured by various stripping
tests
![Page 29: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/29.jpg)
Adhesion and Active Adhesion
Adhesion:"The process of forming chemical bond between the
asphalt film and the aggregate surface”
Active adhesion:"Coating and formation of chemical bond
in the presence of water”
![Page 30: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/30.jpg)
Stripping
Aggregate
"Stripping is the breaking of the bond betweenaggregate and asphalt by the action of water.”
Note about cohesive failure – Pore pressure
Asphalt
![Page 31: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/31.jpg)
General Asphalt Composition- Mixture of Hydrocarbons- Also contain small amounts of acidic and basic
Acid value (mg KOH/g)
Base value (mg KOH/g)
Naphthenic bitumen (Asphalt) 1.5 to 5 0 to 1
Paraffinic bitumen (Asphalt) 0 to 1 0 to 1
Morgan, P., Mulder, A., The Shell Bitumen Industrial Handbook, p 86-88, 1995
organic compounds
![Page 32: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/32.jpg)
Aggregate Type
SurfaceProperties
AsphaltProperties
Quartzite Acidic
Granite AcidicBasic ingredientsusually present
in lesser amountsSandstone Acidic
Limestone Alkaline AcidicIngredients
Aggregate and Asphalt Properties
• Aggregates with a high CaCO3 content will not pass polish test• Fines are siliceous material (sand) and the stripping in the fines
is more of a problem
![Page 33: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/33.jpg)
Stripping in Asphalt PavementsCoating without chemical bonding
Moist Aggregate Dry Aggregate
![Page 34: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/34.jpg)
Osmosis of Water Through Asphalt
• Film thickness• Viscosity• Pressure• Composition of asphalt
Morgan, P., Mulder, A.,The Shell Bitumen Industrial Handbook, 1995
![Page 35: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/35.jpg)
Stripping
![Page 36: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/36.jpg)
![Page 37: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/37.jpg)
Static immersion test at 60°C
![Page 38: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/38.jpg)
Ways to Improve Surface Interaction (Adhesion)
Aggregate
Asphalt
![Page 39: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/39.jpg)
Interaction of Acidic Aggregates and Asphalt With Alkaline Amine
Components - LAS--SiOH + RNH2 --SiO- RN+H3
Polar End Non-Polar Hydrocarbon ChainGroup
H
HN
![Page 40: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/40.jpg)
Asphalt Aggregate Interaction in the Presence of Suitable Compounds in Asphalt
Aggregate
AsphaltChemicalBonding
OH+H2 NSiAnti-StrippingAgentSilicious
Aggregate
Si O H3 N- +
Coating with chemical bonding
![Page 41: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/41.jpg)
Boil Test Results
Aggregate (siliceous)– 20% Type C Gifford Hill– 40% Type D Gifford Hill– 24% Screenings GH– 13% Sand GH– 3% Fines Smithstone
Asphalt– 4.7% Coastal AC-20
Control 0.5% LAS0
20
40
60
80
100% Retained coating
![Page 42: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/42.jpg)
• Mechanical Test– Indirect Tensile Strength
• 50 mm/min. displacement rate• Peak Load at Failure
Tensile Strength
![Page 43: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/43.jpg)
Tensile Strength Ratio Test Results
Control 0.5% LAS0
20
40
60
80
100
120 Dry Str. psi Wet Str. psi%TSR
90% Saturation
![Page 44: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/44.jpg)
Hamburg WheelHamburg Wheel--Tracking TestTracking Test
![Page 45: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/45.jpg)
Material Mix Additive, Cycles Def, BinderID Type % of Asphalt mm
(Granite)Control C ---- 16,000 12.90 PG 76-22LAS C 0.75 20,000 6.40 PG 76-22
(Granite)Control C ---- 14,300 12.50 PG 70-22SLAS C 0.75 20,000 5.60 PG 70-22S
Hamburg WTT Results PavTex Engineering
![Page 46: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/46.jpg)
Typical Test Results, AASHTO T-283
Nova Scotia Granite
0.6
0.7
0.8
0.9
1
1.1
1.2
0 0.1 0.2 0.3 0.4 0.5 0.6 0.7 0.8 0.9 1
Dosage (% by weight of mix)
TSR
LAS 1 LAS 2 Lime
![Page 47: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/47.jpg)
Important test methods for Hot-mixAnd Possible properties evaluatedby various tests
Test Methods Observed Properties
Boil test, Static immersion
Surface interaction betweenaggregate and asphalt (Adhesion)
Lottman type testsAnd Wheel Tracking
tests
Surface interaction (Adhesion)+
Hardening effect of the asphalt and mix (cohesion?)
![Page 48: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/48.jpg)
Observations1. Asphalt Aggregate interaction (Adhesion and
Stripping) depends on the type of aggregate and asphalt composition
2. There is a lack of interaction (Adhesion) in most mixes and can be improved by proper treatment
3. Adhesion and stripping is a surface phenomenon
4. Maybe a combination of stripping tests should be used to evaluate both surface interactions and the mix properties (cohesion?)
![Page 49: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/49.jpg)
AC TO DRUM MIXER
LIQUID ANTI-STRIP LINE
ANTI-STRIP PUMP
HEAT TRANSFER OIL LINES
LAS Injection System
![Page 50: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/50.jpg)
Field System
![Page 51: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/51.jpg)
AC LINE
CUTOFF VALVE
INJECTOR PORT STATIC MIXER
HEATING OIL
HEATING OILFLOWMETER
ANTI-STRIPSTORAGETANK
TEMP.REGULATOR
HEATING OIL
HEATING OIL
STRAINER
Block Diagram
![Page 52: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/52.jpg)
Anti-Stripping Additive Cost Per Ton of Hot Mix
Bitumen, lbs 100
Additive, % 0.5
Additive, lbs/Ton 0.5
Additive cost, $/Ton ~$0.35/TonLAS additive cost a small fraction compared to the
cost of HM (~ 1% of the cost of Hot-Mix)
![Page 53: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/53.jpg)
Benefits of LiquidAnti-Stripping Additives
1. Effective and prolong the life of the pavement
2. Allow wider selection of aggregates3. Inexpensive4. Easy to use
![Page 54: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/54.jpg)
Thank You!
Questions???
![Page 55: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/55.jpg)
![Page 56: Moisture Damage and Benefits of Liquid Anti-stripping](https://reader031.vdocuments.us/reader031/viewer/2022022516/621797194e56b222ee158f3a/html5/thumbnails/56.jpg)