2
The casting of Silver and Brass for the jewellery and costume jewellery market accounts for a large percentage of worldwide production. Costs need to be minimized and Gold Star XL achieves this whilst also producing superior castings and excellent surfaces, keeping finishing work prior to plating to an absolute minimum. Gold Star XL is specifically formulated by optimizing the particle size distribution and thermal expansion to help casters compete in the most demanding of environments for casting Brass and Silver. www.goldstarpowders.com XL GOLD STAR Gold Star XL is a high quality economic gypsum bonded investment powder solution for casting Brass and Silver alloys. Gold Star Powders Spencroft Road, Newcastle-under-Lyme, England ST5 9JE Tel +44 (0)1782 663600 Fax +44 (0)1782 663611 Email [email protected]

Upload: others

Post on 01-May-2022

3 views

Category:

Documents


0 download

TRANSCRIPT

Page 1: GOLD STAR XL - pelusi.com

The casting of Silver and Brass for the jewellery and costume jewellery market accounts for a large percentage of worldwide production. Costs need to be minimized and Gold Star XL achieves this whilst also producing superior castings and excellent surfaces, keeping finishing work prior to plating to an absolute minimum.

Gold Star XL is specifically formulated by optimizing the particle size distribution and thermal expansion to help casters compete in the most demanding of environments for casting Brass and Silver.

www.goldstarpowders.com

XLGOLD STAR

Gold Star XL is a high quality economic gypsum bonded investment powder solution for casting Brass and Silver alloys.

Gold Star PowdersSpencroft Road, Newcastle-under-Lyme, England ST5 9JE

Tel +44 (0)1782 663600 Fax +44 (0)1782 663611 Email [email protected]

Page 2: GOLD STAR XL - pelusi.com

www.goldstarpowders.com

Gold Star PowdersSpencroft Road, Newcastle-under-Lyme, England ST5 9JE

Tel +44 (0)1782 663600 Fax +44 (0)1782 663611 Email [email protected]

Gold Star XL is available in 22.5kg sacks

Do not remove flasks from furnace to cast until they have been held at casting temperature for a minimum of 1 hour. If held for less than 1 hour, the core of the flasks will be at a much higher temperature than the digital temperature display states, and may result in metal mould reaction.

• Do no not cast with a flask temperature lower than 650°C• Slurry temperature 21°C• Leave for 90 min to stand before burnout

WATER TO POWDER RATIO

MACHINE VACUUM MIXING 38:100

HAND MIX THEN VACUUM 40:100

XLGOLD STAR

MIXING INSTRUCTIONSPOWDER TO WATER RATIO 100 TO 38

MIXING BY HAND MIXING BY MACHINE

1 Add powder to water 1 Add powder to water

2 Mix for 3 minutes 2 Mix for 4 - 5 minutes under full vacuum

3 Vacuum mixture for 1 minute 3

4 4 Vacuum flasks for 2 minutes

5 Vacuum flasks for 2 minutes 5 Remove flasks immediately from vacuum and to stand on a firm surface for 2 hours

6Remove flasks immediately from vacuum and to stand on a firm surface for 2 hours

SRS PRODUCT SELECTOR CHART

Bras

s

Silve

r

9k Y

ello

w

12k

Yello

w

14k

Yello

w

18k

Yello

w

22k

Yello

w

9k W

hite

14k

Whi

te

18k

Whi

te

Silk

Classic

Eurovest

Time in hours

0

100

200

300

400

500

600

700

800

71 82 93 104 115 126 13 14

730°C

230°C

150°C/hr

1.5hrs 3hrs 3.5hrs 4hrs 1hr

Tem

pera

ture

°C

BURNOUT CYCLE

MACHINE VACUUM MIXING Min.

Weigh out water and powder 0

Add powder to water 0

Mix under vacuum 5

Pour flasks 2

Vacuum flasks 1

Total time take 8

HAND MIX THEN VACUUM Min.

Weigh out water and powder 0

Add powder to water and mix 4

Vacuum mixer bowl 1

Pour flasks 1

Vacuum flasks 2

Total time taken 8