N. Pinna | 18.01.2013
Atomic Layer Deposition
Nicola Pinna
Humboldt-Universitt zu Berlin, Institut fr Chemie, Brook-Taylor-Str. 2, 12489Berlin, Germany
E-mail: [email protected]
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
2/68
N. Pinna | 18.01.2013
Outline of the Presentation
1. Literature2. Introduction to Atomic Layer Deposition
3. Chemistry in ALD
4. ALD Reactors
5. Nanostructures
6. Applications
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
3/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
4/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
5/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
6/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
7/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
8/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
9/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
10/68
N. Pinna | 18.01.2013
Progress and future directions for
atomic layer deposition and ALD-based
chemistry. This issue of MRS Bulletin
details current progress in atomic layer
deposition, including the extension of ALDto new regions of the periodic table, and
molecular layer deposition and vapor in
filtration for synthesis of organic based thin
films. The cover image shows a diagram of
an ALD reaction schemea snapshot of the
reactants and products as they would be
flowing from left to right. This is a general,
stylized ALD reaction scheme to visualize
surface ligand exchange. The backgroundis a scanning electron microscopy image of
2 nm ALD-deposited Pt nanoparticles
uniformly dispersed on strontium titanate
nanocubes.
MRS Bulletin / Volume 36 / Issue 11 / November 2011, pp 899-906
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
11/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
12/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
13/68
N. Pinna | 18.01.2013
Atomic Layer Deposition
ALD is a method for depositing thin films onto various substrates withatomic scale precision.
The principle is similar to chemical vapor deposition (CVD), except thatthe ALD reactions are separated into two half-reactions by keeping the
precursor materials separate during the reaction.
ALD film growth is self-limited and based on surface reactions.Therefore, film thickness control can be as fine as one monolayer.
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
14/68
N. Pinna | 18.01.2013Riikka L. Puurunen, J. Appl. Phys., 2005, 97, 121301
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
15/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
16/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
17/68
N. Pinna | 18.01.2013
Short History
1970s - The ALD technology was developed in Finland and patented.Technology for thin films electroluminescent (TFEL) flat panel display.Suntola, T. and Antson, J., Method for producing compound thin films, USPatent 4 058 430 (1977).At that time the technique was called Atomic Layer Epitaxy (ALE)
TFEL displays commercialized in 1980 were based on ALDAl2O3/ZnS:Mn/Al2O3 structures
Ein Flughafendisplay, dessen elektrolumineszenteBeschichtung durch das ALD-Verfahren hergestellt
wurde. Das Verfahren wurde fr diesen Zweck Endeder siebziger Jahre entwickelt.
Source: http://www.weltderphysik.de/gebiete/stoffe/duenne-schichten-und-oberflaechen/atomic-layer-deposition/
Source: http://lumineq.com/en/technology
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
18/68
N. Pinna | 18.01.2013
Short History
Mid-1980s to the mid-1990s - The ALD research was extremely active onthe epitaxial growth of III-V, II-VI, Si and Ge semiconductors
Beginning of the 21th-century- Microelectronic industry drives thedevelopment of the ALD due to the continuous scaling of microelectronicdevices1st application: ALD of Al2O3 insulating layers in DRAM capacitors due tothe need of rather thin and conformal coating of high aspect ratio
structures2007: Intel announces the use of HfO2-based high- gate oxides in CMOStransistors ALD
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
19/68
N. Pinna | 18.01.2013
Intel in 2007 introduced ALD of Hf-based oxide in 45 nm technology
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
20/68
N. Pinna | 18.01.2013http://nano.tkk.fi/en/research_groups/microfabrication/research/microfabrication/
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
21/68
N. Pinna | 18.01.2013
Introduction to the Chemistry Employed in ALD
Oxides: Hydrolysis-Condensations Oxygen sources (H2O, H2O2, O3,...)
Nitrides: Aminolysis (e.g. NH3)
Sulfides: Sulfur, Hydrogen sulfide
Metals: O
2, H
2, etc.
Requirements for the precursors: Reasonably high vapor pressure in order to allow saturation of the chambervolume upon dosing Good thermal stability to avoid decomposition prior to the next step Must chemisorb onto the substrate to be coated
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
22/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
23/68
N. Pinna | 18.01.2013
Metal Precursors
M. Putkonen, Chapter 3: Precursors for ALD Processes
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
24/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
25/68
N. Pinna | 18.01.2013
Basic hydrolysis of alkoxysilanes (SN2)
Acid hydrolysis of alkoxysilanes (proton assisted SN1)
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
26/68
N. Pinna | 18.01.2013
Polycondensation
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
27/68
N. Pinna | 18.01.2013
Silica Growth in ALD: Base Catalyzed
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
28/68
N. Pinna | 18.01.2013
Silica Growth by ALD: Self-Catalyzed
a) Anchoring: surface hydroxygroups cleave Si-OEt bonds ofthe silane under self-catalysis bythe pendent amino group (green),causing chemisorption
b) Hydrolysis: remaining ethoxygroups are removed self-catalytically
c) Oxidation: the aminoalkyl armis removed by ozone
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
29/68
N. Pinna | 18.01.2013
Platinum thin films were grown at 300 C by atomic layer deposition (ALD) using(methylcyclopentadienyl)trimethylplatinum (MeCpPtMe3) and oxygen as precursors. Thefilms had excellent uniformity, low resistivity, and low-impurity contents.
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
30/68
N. Pinna | 18.01.2013
Plasma-enhanced ALD
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
31/68
N. Pinna | 18.01.2013
Plasma-enhanced ALD
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
32/68
N. Pinna | 18.01.2013
Molecular Layer Deposition
Illustration of surface chemistry forPPTA MLD using terephthaloyl chlorideand p-phenylenediamine as reactants.
S.M. George, B. Yoon, A.A. Dameron; Acc. Chem. Res. 2009, 42, 498-508.
Illustration of surface chemistry forpoly(aluminum ethylene glycol) aluconeMLD using TMA and EG as reactants.
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
33/68
N. Pinna | 18.01.2013
1. Nonhydrolytic Hydroxylation Reactions(Formation of M-OH species)
Reaction of alcohols with metal halides:
1) Coordination of the alcohol to the metal centre
2) a) Formation of metal alkoxide under elimination of HX
b) Formation of hydroxyl group and elimination of alkyl halide RX(if R is an electron-donor substituent, the nucleophilic attack ofthe chloride on the carbon group is favored)
A. Vioux: Chem. Mater. 1997, 9, 2292-2299
Nonaqueous Sol-Gel Routes to Oxides
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
34/68
N. Pinna | 18.01.2013
Aprotic Condensation Reactions
(M-O-M Bond Formation)
A. Vioux: Chem. Mater. 1997, 9, 2292-2299
Reaction between two metal alkoxides under ether elimination
Reaction between metal acetates and metal alkoxides under ester elimination
Reaction between metal alkoxides and metal halides under alkyl halide elimination
Nonaqueous Sol-Gel Routes to Oxides
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
35/68
N. Pinna | 18.01.2013
Alkyl Halide Elimination
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
36/68
N. Pinna | 18.01.2013
M-OR + RCOOH M-OOCR + ROH Eq. 1
M-OOCR + M-OR
M-O-M
+ RCOOR Eq. 2
Non-Aqueous Sol-Gel Routes Applied to ALD
Angew. Chem. Int. Ed. 2008, 47, 3592 - J. Phys. Chem. C 2008, 112, 12754,J. Mater. Chem. 2009, 19, 454 - Adv. Funct. Mater. 2011, 21, 658Patent WO 2008 098963 A2
Low oxidative character of carboxylic acids Large deposition temperature range
High quality and purity of the films No OH groups involved in the M-O-M bond formation
Metal Precursors: Hf(OtBu)4, Ti(OiPr)4, VO(OPr)3, Sn(OtBu)4 Oxygen Sources: Carboxylic acids e.g. acetic acid Deposition temperature: 50 350 C
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
37/68
N. Pinna | 18.01.2013
3rd TIP 2nd Ac.
3rd Ac. 3rd TIP
Ti-OCCD3
SiH
CH
10001500200025003000 Wavenumbers (cm-1)
COO
3rd cycle
14th cycle
Difference FT-IR spectra
14th TIP 13th Ac.
14th Ac. 14th TIP
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
38/68
N. Pinna | 18.01.2013
TiO2
Self-limiting growth!
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
39/68
N. Pinna | 18.01.2013
ALD Reactors
Copyrighted Content Removed
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
40/68
N. Pinna | 18.01.2013
Copyrighted Content Removed
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
41/68
N. Pinna | 18.01.2013
Copyrighted Content Removed
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
42/68
N. Pinna | 18.01.2013
Compact Reactors
Copyrighted Content Removed
B h
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
43/68
N. Pinna | 18.01.2013
Various types of typical ALD reactor systems. a) Cross-flow reactorsystem based on forced flow laterally across the wafer. b) systemwith single injector above the center of the wafer. c) shower headsystem; gas is injected through an array of injectors covering theentire wafer surface. d) Vertical batch reactor: 50150 wafers areprocessed simultaneously.
Batch Reactors
E. Granneman, P. Fischer, D. Pierreux, H. Terhorst, P. Zagwijn, Surf.Coatings Technol. 2007, 201, 8899
Copyrighted Content
Removed
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
44/68
N. Pinna | 18.01.2013
J. Meyer and T. Riedl. Chapter 6: Low-Temperature Atomic Layer Deposition
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
45/68
N. Pinna | 18.01.2013
Fluidized bed reactor Rotary reactor
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
46/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
47/68
N. Pinna | 18.01.2013
Fabrication of Nanostructures
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
48/68
N. Pinna | 18.01.2013
Nature Mater. 2006, 5, 627.
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
49/68
N. Pinna | 18.01.2013
Conformal coating of carbon nanotubes
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
50/68
N. Pinna | 18.01.2013
HfO2TiO2
VOx
Carbon nanotube
TiO2
VOx
SEM images recorded at
different accelerationvoltages using SE and BSEdetectors prove that thetubes are coated on the in-and outside surfaces.
Characterization:SEM
Nano Lett. 2008, 8, 4201 - Phys. Chem. Chem. Phys. 2009, 11, 3615 - Adv. Funct. Mater. 2011, 21, 658
Conformal coating of carbon nanotubes
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
51/68
N. Pinna | 18.01.2013
Characterization:HRTEM
High resolution imagingshows the amorphous
character of the asdeposited films.However, in the case ofVxOy films, annealing at150C induces
crystallization (V2O5).
HfO2 TiO2
VOx VOx after annealing @ 150C
Chemical Analysis
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
52/68
N. Pinna | 18.01.2013
Characterization: Electron Energy Loss Spectrometry (EELS)
Chemical Analysis
Effect of the CNTs functionalization
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
53/68
N. Pinna | 18.01.2013
Effect of the CNTs functionalization
J. Mater. Chem. 2012, 22, 7323
Effect of the CNTs functionalization
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
54/68
N. Pinna | 18.01.2013
Effect of the CNTs functionalization
J. Mater. Chem. 2012, 22, 7323
Applications in Energy Related Fields
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
55/68
N. Pinna | 18.01.2013
pp gy
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
56/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
57/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
58/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
59/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
60/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
61/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
62/68
N. Pinna | 18.01.2013
Gas Sensors
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
63/68
N. Pinna | 18.01.2013
3 mm
6mm
3 mm
6mm
Front sidegold electrodes
Back sideplatinum contacts
Cross section
0.3
8
mm
Alumina substrate
Sensing layer
50 m
Angew. Chem. Int. Ed. 2004, 43, 4345
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
64/68
N. Pinna | 18.01.2013Nano Lett. 2008, 8, 4201 - Phys. Chem. Chem. Phys. 2009, 11, 3615 - Adv. Funct. Mater. 2011, 21, 658
SnO2 coated CNTs
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
65/68
N. Pinna | 18.01.2013
0 1000 2000 3000
40
42
44
46 a)
Time (sec)
Resistance()
NO2in
NO2out
Pure CNTs are p-type semi-conductors SnO2 coated CNTs are n-type semiconductors
formation of a p-n heterojunctionbetween the metal oxide film and support
Nano Lett. 2008, 8, 4201 - Adv. Funct. Mater. 2011, 21, 658
0 200 400 600 80010
4
10
5
Resistance
()
Time (sec)
5 ppm NO2
NO2 in
NO2 out
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
66/68
N. Pinna | 18.01.2013
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
67/68
N. Pinna | 18.01.2013
Oxidative dehydrogenation of ethane toethylene at 650 C
SCIENCE, 2012, 335,1205
-
8/10/2019 Nicola Pinna Atomic Layer Deposition 130118
68/68
N. Pinna | 18.01.2013NATURE CHEMISTRY, 2012, 4, 1031