Lead-Free Inspection Methods
Tom PerrettMarketing Manager – Soldertec
&Keith Bryant
European Sales Manager – Dage Precision Industries
![Page 2: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/2.jpg)
©
Overview
Look at the solder!!ICP 610DLead detection fluidsMicrosectioning & SEMX-ray inspectionXRF (also detects Cd, Hg, Cr, Br)Conclusions & Questions
![Page 3: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/3.jpg)
©
Which are lead-free?
![Page 4: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/4.jpg)
©
Look at the solder
Is the products labelled?Understand the codes for the alloys e.g. Sn/Pb, SAC, Sn/Bi, 305Feel the solder. Is it easy to bend?Lead-free solder paste often has a slight greenish appearance in the jar.
![Page 5: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/5.jpg)
©
Different ways of saying lead-free
SAC305Sn/Ag/Cu96.5% Sn/ 3.0%Ag/ 0.5%Cu
96SCIt says Tin Silver CopperUS pat…………..may be different to first reel.
![Page 6: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/6.jpg)
©
![Page 7: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/7.jpg)
©
Lead Free additions to J-STD-001 and IPC – A- 610
Lead Free--610 chapter 5 first few pagesIPC/J-STD-001 clause 14. There is NO DIFFERENCE in the solder connection fillet requirements.
There are some differences in superficial appearance
![Page 8: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/8.jpg)
©
Lead Free Solder joint requirements
The primary difference is related to the visual appearance of the solder. Acceptable lead-free and tin-lead connections may exhibit similar appearances but lead free alloys are more likely to have:
Surface roughness (grainy or dull).Different wetting contact angles.
All other solder fillet criteria are the same.
![Page 9: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/9.jpg)
©
Solder joint Acceptable - Class 1,2,3
There are materials and processes, e.g. lead free alloys and slow cooling with large mass PCBs, that may produce dull matte, gray, or grainy appearing solders that are normal for the material or process involved. These solder connections are acceptable.Wetting contact angle of 90o or less, except when the quantity of solder results in a contour which extends over the edge of the solderable surfaces or solder resist
![Page 10: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/10.jpg)
©
Lead versus Lead Free – No Clean
![Page 11: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/11.jpg)
©
Lead vs. lead free – Water Soluble Flux
![Page 12: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/12.jpg)
©
Flat pack Water Soluble flux
![Page 13: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/13.jpg)
©
BGA No Clean
![Page 14: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/14.jpg)
©
Special Lead free requirements
5.2.10 Soldering Anomalies – Lead FreeAcceptable lead free connections may exhibit:- Fillet lifting - separation of the bottom of the solder and the top of the land - Shrink holes, fissures or hot tearing
![Page 15: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/15.jpg)
©
BGA VoidingDesign induced voids, e.g., microvia in land, are excluded from this criteria. (manufacturer/user discussion)Manufacturers may use test or analysis to develop alternate acceptance criteria for voiding that consider the end-use environment.
Acceptable - Class 1,2,3• 25% or less voiding of the ball x-ray image area.Defect - Class 1,2,3• More than 25% voiding in the ball x-ray image area.
![Page 16: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/16.jpg)
©
BGA Voiding Controversy
Controversy: Why 25% and not 35%? IPC-A-610 committee was provided data that established acceptability of 25% figure. Did not have data regarding higherlevels even though these might be okay.
![Page 17: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/17.jpg)
©
Lead-Free Surface Testing
![Page 18: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/18.jpg)
©
NPL Reported
4 test kits tested3 failed to detect lead in a 40% lead solder terminationThe successful kit failed to detect lead at 15% in further tests.
![Page 19: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/19.jpg)
©
Can you see the difference?
![Page 20: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/20.jpg)
©
Now you can!!
![Page 21: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/21.jpg)
©
Lead-free Solder
Still have IMLVoiding still possibleWetting similar
![Page 22: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/22.jpg)
©
X-ray inspection
![Page 23: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/23.jpg)
©
Popcorning in BGAs
From IPC7095ASection 7.5.7 – “…popcorning and warpage are generally caused by improper handling of the BGA component prior to reflow. Popcorning causes the BGA package to expand below the die; resulting in an increase in size (and possibly bridging) of the solder balls in the center of the package as they are squished between the package and the board.”
![Page 24: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/24.jpg)
©
Moisture Sensitivity Levels
< 30oC/85%RHTime on label6
< 30oC/85%RH24 hours5a
< 30oC/85%RH38 hours5
< 30oC/85%RH72 hours4
< 30oC/85%RH168 hours3
< 30oC/85%RH4 weeks2a
< 30oC/85%RH1 year2
< 30oC/85%RHUnlimited1
Floor ConditionFloor TimeLevel Indicator
Outlined in IPC/JEDEC J-STD-020COutlined in IPC/JEDEC J-STD-020C
![Page 25: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/25.jpg)
©
BGA Opens Using Digital X-ray Inspection
BGABGABGA
BallBallBall
Solder PasteSolder PasteSolder Paste
PadPadPad
PCBPCBPCB
2 ellipses on the x-ray image show BGA connection are OK
2 ellipses on the x2 ellipses on the x--ray ray image show BGA image show BGA connection are OKconnection are OK
PadPad
PCBPCBPCB
Solder PasteSolder PasteSolder Paste
BGABGABGA
BallBallBall Missing ellipse indicates open jointMissing ellipse indicates Missing ellipse indicates open jointopen joint
![Page 26: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/26.jpg)
©Interfaces in BGA Joints
![Page 27: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/27.jpg)
©
LeadLead--free CSP Imagefree CSP Image
Open ConnectionOpen Connection
![Page 28: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/28.jpg)
©
Missing ellipse can indicate open jointsVery subtle greyscale differencesLocation of void with respect to interface is very clear
![Page 29: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/29.jpg)
©
Angled view showing voids, partial joints and Angled view showing voids, partial joints and solder ballingsolder balling
![Page 30: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/30.jpg)
©
Oblique-view - you can see the BGA and Land pad clearly and PCB connection crack
BGA Size (350um)BGA Size (350um)
![Page 31: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/31.jpg)
©
Flip chip inside plastic BGA, showing ball damage
caused by excessive heat
![Page 32: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/32.jpg)
©
Oblique angle Digital image showingOblique angle Digital image showingboth joint interfaces with some voiding,both joint interfaces with some voiding,plus ball cracking caused by excessive heatplus ball cracking caused by excessive heat
![Page 33: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/33.jpg)
©
BGA ballBGA ballescapingescapingdown a viadown a via
![Page 34: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/34.jpg)
©
CapacitorCapacitorCrackingCracking
![Page 35: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/35.jpg)
©
PIHR Insufficient FillPIHR Insufficient Fill
![Page 36: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/36.jpg)
©
Voiding &Voiding &Poor WettingPoor Wetting
![Page 37: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/37.jpg)
©
Voids and misalignmentVoids and misalignment
![Page 38: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/38.jpg)
©
Heel Voids under Joints
![Page 39: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/39.jpg)
©
Outgoing QA InspectionOutgoing QA Inspection
ICT / AOI are not able to spot this defect but XICT / AOI are not able to spot this defect but X--ray canray can
Excessive voidsExcessive voids
![Page 40: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/40.jpg)
©
Die Attach Cracks causedDie Attach Cracks causedby Reflow Temperatureby Reflow Temperature
![Page 41: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/41.jpg)
©
What is being restricted by RoHS?
LeadMercuryCadmiumChromium (vi)PBB (Polybrominated biphenyls)PBDE (Polybrominated diphenyl ethers)
All restricted to 1000ppm, except Cd which is 100ppm
Risks to health include damage to liver and central nervous system, birth defects, carcinogens & endocrine distruption.
![Page 42: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/42.jpg)
©
RoHS: Impurity Limits
Maximum Concentration Values in weight percent- 0.1% for Pb, Hg, hex. Cr- 0.01% for Cd- 0.1% for PBB and PBDE flame retardants
Concentration is per homogeneous material
‘Homogeneous material means a material that cannot be mechanically disjointed into different materials’
![Page 43: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/43.jpg)
©
Example of Materials......
lead-framelead-frame
coating
solder
copper board finish
board surface finish
copper
glassepoxy
![Page 44: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/44.jpg)
©
Where banned substances might be?
Mechanical fixings – may be Zn plated with hexavalent Cr used as a passivation layer
Plastics – may contain Pb, Cd or PBDE
Components – may have Pb on surface finish or as internal connections
Etc !
![Page 45: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/45.jpg)
©
Analysis techniques - examples
Technique Substances Comments
AAS Pb, Cd, Hg, total Cr Dissolve components or material
ICP Pb, Cd, Hg, total Cr Dissolve components or material
ED-XRFA Pb, Cd, Hg, total Cr and Br
Useful surface analysis method –has limitations
SEM-EDX Pb, Hg, total Cr and Br
Surface analysis – useful for very small features but has limitations
Visible spectroscopy
Hexavalent Cr Dissolve coating to form coloured solution
GCMS PBB & PBDE Various options
DTI Report Compliance, 2004
![Page 46: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/46.jpg)
©
![Page 47: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/47.jpg)
©
![Page 48: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/48.jpg)
©
Banned Substances
Pb in solders, PCB finishes, component terminations.Hg in Switches, lamps, thermostats & sensorsCd in switches, springs, pigments, housings & batteriesCr(VI) as anticorrosion coating and wood preservativesBrominated flame retardants in casings (59%), PCBs (30%), connectors & relays (9%), wire & cable (2%)
Don’t just think of electronic circuits….think about the whole product; including cables, screws, housing, plugs etc
![Page 49: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/49.jpg)
©
WHAT IS IN OUR OLD PRODUCTS?
3 to 8 years old
No cadmium or mercury. BT banned Cd in 1997Lead weights
Lead solder
Bromine based flame retardants
Hexavalent chrominum on screws and speaker mount
Lead in PVC
![Page 50: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/50.jpg)
©
WHAT IS IN OUR OLD PRODUCTS?
Hexavalent chromium on screws
Lead solder and Bromine based flame retardants
1 to 3 years ago
No cadmium or mercury in product.
No lead stabilisers in cordage
No lead weights
![Page 51: Lead-Free Inspection Methods](https://reader031.vdocuments.us/reader031/viewer/2022012410/616a5bf711a7b741a351a303/html5/thumbnails/51.jpg)
©
Conclusions
Lead-free solder joints look subtly different, IPC-A-610DNeed to control materials used on site between RoHS compliant and non-compliantAs solder joints become smaller X-ray inspection plays an ever more important role in inspection.Tests are available to screen for compliance.Once compliant; records need to be kept for 4 years.