![Page 1: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/1.jpg)
Hotwire-assisted Atomic Layer Deposition of Pure Metals and
Metal Nitrides
1
Alexey Kovalgin
MESA+ Institute for NanotechnologySemiconductor Components group
![Page 2: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/2.jpg)
Motivation
2
CMOS backend:seed layers & barriers
Multi-gate transistor
Group III – Nitride TFTs
High aspect ratio structures
(e.g. memories)(S. Bolat et al. Appl. Phys. Lett.
2014)
1. Materials 2. Deposition method
(chipworks.com)
(chipworks.com)
(chipworks.com)
![Page 3: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/3.jpg)
3
TiCl4TiCl4TiCl4TiCl4HClHCl
NH3NH3
Classic example of thermal ALD
NH3NH3HClHCl
HClOTiClTiClOH +−→+− 34
HClTiNHNHTiCl +−→+− 23
Courtesy of Hao Van Bui
Metallic TiN filmsALD: Self-limiting reactions Thickness control High aspect ratio
structures
![Page 4: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/4.jpg)
4
NH3NH3
Need for extra activation
XM
CH3
CH3
XC
H HH
M(CH3)3
XM
CH3
CH3
XC
H HH
H H
NH H
NH H
CH4
Readily occurs for Al, difficult for Ga
M = Al, Ga
ALD of AlN and GaN compared
![Page 5: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/5.jpg)
5
Plasma-Enhanced ALD (PEALD)1st precursor: plasma off
2nd precursor: plasma on
![Page 6: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/6.jpg)
6
ALD classification
Thermal Radical-Enhanced
Atomic Layer Deposition
Purpose: Hot-wire generated radicals (H, NHx, …) for ALD w/o plasma
Joe N. Smith and Wade L. Fite, J. Chem. Phys. 32, 898, (1962)
Cat. dissociation of H2 on hot tungsten filament
PEALD Making radicals w/o plasma?
![Page 7: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/7.jpg)
7
1. Breaking molecules by electrons or excited species
2. Number of chemical reactions can be significant
3. Ions are present => more reactions & charging
4. UV light emission
1. Catalytic dissociation by a hot (1600-2000 oC) tungsten wire
2. Lower pressures possible
3. Number of reactions is limited
4. No ions
5. No UV
Plasma Hot Wire
Plasma versus Hot Wire
7
![Page 8: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/8.jpg)
8
Outline
Motivation
Hotwire-Assisted Deposition: Confirmation of the Presence of Atomic Hydrogen
HWALD of Tungsten (W) Films
On the Growth of Titanium (Ti) Films
Confirmation of the Presence of Nitrogen radicals
On the Growth of Aluminum Nitride (AlN) Films
Conclusions
Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides
![Page 9: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/9.jpg)
9
HWALD: Which radicals can be formed?Confirmation of the Presence of Atomic Hydrogen
Topic of the presentation
![Page 10: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/10.jpg)
10
Reactor details
Reactor 2
Substrate
Inner reactor
EllipsometerHot-wire “chimney”A. Y. Kovalgin, and A. I. I.
Aarnink, US Patent 20130337653 A1, 2013.
![Page 11: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/11.jpg)
11
Is at-H delivered to the wafer surface?
Atomic hydrogen reacts with Te surface producing TeH2:
2H + Te(s) TeH2(g) etching Te film
There is no reaction between molecularhydrogen and Te.
![Page 12: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/12.jpg)
12
Real-time monitoring of Te etchingThe etching of Te was real-time monitored by in-situ SE(1) Introducing H2, FILAMENT OFF(2) Stop introducing H2, heat up the filament(3) Introducing H2 with FILAMENT ON
100 nmSubstrate
Te
Thickness verification by SEM
H. Van Bui et.al., ECS J. Solid State Sci. Technol. 2
(4) P149-P155 (2013).
![Page 13: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/13.jpg)
Etching of Te by H-pulses
13
Bridge to Hot Wire ALD (HWALD)
H. Van Bui et al.: ECS journal of solid state science and technology 2 (4) P149-P155 (2013).
![Page 14: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/14.jpg)
~70 L
Reactor 1
14
Delivering atomic-H goes easily
few ml
Reactor 2
few ml
Reactor 3
Horizontal HW
H2,NH3
Wafer
Vertical HW(line-of-sight)
H2, NH3
Wafer
Adv. Mater. Interfaces 2017, 1700058
![Page 15: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/15.jpg)
15
HWALD of Tungsten (W) Films
Topic of the presentation
![Page 16: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/16.jpg)
In-situ SE monitoring
Stopping pulses here
Starting pulses here
27
• Sequential pulses of WF6 and at-H• Well-defined ALD window can be found
One ALD cycle:
1. at-H2. Purge3. WF64. Purge
![Page 17: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/17.jpg)
Properties of W
17
High purity
Excellent step coverage
Yang et al., Thin Solid Films, https://doi.org/10.1016/j.tsf.2017.12.011
![Page 18: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/18.jpg)
Crystallinity
18
Yang et al., Thin Solid Films, https://doi.org/10.1016/j.tsf.2017.12.011
![Page 19: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/19.jpg)
Resistivity
19
14.8
15.2
14.9 15.0 15.0
µΩ·cm
Film thickness: 10-12 nmRMS: 1.4 nm
Resistivity: • 100 µΩ·cm, β-phase• 15 µΩ·cm, α-phase
Ω·cm
Resistivity mapping
14.7
14.9
15.0
15.1
15.2
15.315.5
Yang et al., Thin Solid Films, https://doi.org/10.1016/j.tsf.2017.12.011
![Page 20: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/20.jpg)
20
HWALD: On the Growth of Titanium (Ti) Films
Topic of the presentation
![Page 21: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/21.jpg)
Reference: ALD of TiN by TiCl4/NH3 pulses
21
1 cycle
50% N46% Ti4% O
H. Van Bui, A. Y. Kovalgin, and R. A. M. Wolters. ECS journal of solid state science and technology 1 (6) P285-P290 (2012).
![Page 22: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/22.jpg)
0 10 20 30 40 50 60 70 800
10
20
30
40
50
60
70
80
90
100110801010.pro
Sputter Depth (nm)
Atom
ic C
once
ntra
tion
(%)
N1sSi2pO1sTi2p
43 at.% Ti
Surface passivation by a-Si
25 at.% N
35 at.% O(was 3-5 %)
22
TiCl4/H/NH3 pulses
Atom
ic c
once
ntra
tion
(%)
Sputter depth (nm)
Base pressure 2×10-7 mbar
Arrival of contaminants: 0,1 monolayer/s
H. Van Bui et al.: ECS journal of solid state science and technology 2 (4) P149-P155 (2013).
![Page 23: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/23.jpg)
TiCl4/H pulse sequence H reduces –Cl groups, releasing HCl and leaving
dangling bonds…
23
TiO-HH-O
TiO
Ti
ClClCl
Cl
Ti
ClClCl
Cl
Case #1: H atoms occupy dangling bonds Would be great…
but: 10-7 mbar of residual H2O
Case #2: O atoms occupy dangling bonds
TiO2 will continue growing but very slowly as it is limited by the supply of H2O
TiHH
Ti
Ti
ClClCl
ClH
Ti
ClClCl
Cl
![Page 24: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/24.jpg)
24
Topic of the presentation
It does work for W… Why not for Ti, Al, …?
![Page 25: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/25.jpg)
25
HWALD: Which radicals can be formed?
On the Presence of Nitrogen Radicals
Topic of the presentation
![Page 26: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/26.jpg)
26
N-radicals delivered in line of sightHorizontal HW
NH3
Wafer
Vertical HW(line-of-sight)
NH3
Wafer
0 30 60 900,0
0,1
0,2
0,3
0,4
0,5
Thic
knes
s (n
m)
Time (min)
HW off HW horizontal HW vertical
NitridizingSi wafer
Real-time SE acquisition
Adv. Mater. Interfaces 2017, 1700058
![Page 27: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/27.jpg)
N
Al
O
Towards AlN: HW out of line-of-sight
27
Horizontal HW
NH3
Wafer
0 5 10 15 200
20
40
60
80
100
Atom
ic %
Sputter time (min)
HW on
N
Al
OSi
HW off
Adv. Mater. Interfaces 2017, 1700058
350 oC
![Page 28: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/28.jpg)
28
NH3Vertical HW(line-of-sight)
Wafer
Adv. Mater. Interfaces 2017, 1700058Towards AlN: HW in line-of-sight
350 oC
![Page 29: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/29.jpg)
ALD = self-limiting surface reactions => advantages Additional means to supply energy sometimes required HW can (to some extent) replace plasma: Generation of at-H confirmed by etching of Te films
at-H: delivery in both in and out of line-of-sight possible
Generation of Nitrogen radicals confirmed by nitridation of Si
Nitrogen radicals: delivery in line-of-sight only
Obviously (residual) oxidants can also be activated by HW
Metal oxidation and reduction of the oxides should be taken into account
HWALD enables (so far): Area-selective growth of high-qiality W using WF6/at-H
Deposition of TiOx using TiCl4/at-H
Deposition of AlNyOz using TMA and NH3 via HW
29
Conclusions
![Page 30: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/30.jpg)
Many thanks to: Mengdi Yang (PhD student – HWALD W)
Sourish Banerjee (PhD student – AlN/GaN ALD)
Hao Van Bui (graduated PhD student – Te etching, TiN ALD)
Ramazan Oguzhan Apaydin (PhD student – BN)
Tom Aarnink (technical support of deposition tools)
Rob Wolters (discussions)
Jurriaan Schmitz (discussions)
Dirk Gravesteijn (discussions)
Mark Smithers, Gerard Kip (MESA+) for SEM and XPS analyses.
This work is financially supported by the Netherlands Organization for Scientific Research (NWO) and ASM International.
30
![Page 31: Hotwire-assisted Atomic Layer Deposition of Pure Metals and … · 2017-12-27 · Hotwire-assisted Atomic Layer Deposition of Pure Metals and Metal Nitrides 1 Alexey Kovalgin MESA+](https://reader030.vdocuments.us/reader030/viewer/2022040815/5e5bf80e6a18dd284c16d9bd/html5/thumbnails/31.jpg)
Thank you for your attention!