adaptive control - welding technology corporation
TRANSCRIPT
![Page 1: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/1.jpg)
David Androvich & Ellis Mayton
AWS SMWC Tutorial, October 16, 2018
![Page 2: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/2.jpg)
2
1. What is Adaptive Control?
2. Resistance’s Relationship to Quality
3. Importance of the Resistance Curve
4. The Reference Weld
5. Real Time Adaptive Decisions
6. Implementing Adaptive Control
7. Adaptive vs. Constant Current Control
8. Conclusion
1
2
3
4
5
6
7
8
![Page 3: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/3.jpg)
3
A tool to analyze welding data and make intelligent corrections based on that analysis.◦ The analysis is based on an input of a new variable(s)
supplied to the weld control that is related to nugget diameter.
Steel – Dynamic Resistance obtained by secondary tip wires
Aluminum – Dynamic Force obtained by strain or load cells in the gun
◦ The corrections are automatically made to weld current and/or weld time during the weld schedule.
1
![Page 4: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/4.jpg)
4
Adaptive control is not:◦ A tool to solve impossible weld problems. If you can not
make a good constant current weld you generally can not make a good adaptive weld.
◦ A tool that will operate forever without normal weld and tooling maintenance.
There are two types of adaptive controls:◦ Those that rely on internal algorithms to make adjustments.
◦ Those that use a stored “reference weld” and algorithms to make adjustments. These types generally have a better ability to adjust for disturbances.
1
![Page 5: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/5.jpg)
5
Adaptive controls are designed to compensate for the following levels of production disturbances:◦ Material thickness and composition variations
◦ Electrode wear (without using steppers)
◦ Weld force variation
◦ Gun fit up
◦ Expulsions
◦ Sealers
◦ ……Etc
When Adaptive controls sense an inability to compensate for a disturbance, a new series of alerts/alarms are generated.
1
![Page 6: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/6.jpg)
6
The heat generated at the faying resistance creates the nugget.
[1]
𝑯𝒆𝒂𝒕 = 𝑰𝟐 ∙ 𝑹 ∙ 𝒕 𝑹 ∝𝝆 ∙ 𝒍
𝑨
[2]
Molten Region
2
![Page 7: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/7.jpg)
The bulk & contact resistance values fluctuates during the weld as a result of the mechanisms of nugget formation.
7
[3]
2
The total dynamic resistance observed during RSW is the sum of:
• Contact resistance between the metal sheets (faying surface
• Bulk resistance of the metal sheets
• Contact resistance between the electrodes and sheets
• Bulk resistance of the electrodes and the electrode holders
![Page 8: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/8.jpg)
The dynamic resistance curve can take on a variety of shapes, but will generally exhibit 3 phases.
The data from the curve provides quality indicators for the weld.
8
1. Coupling
2. Heating/Melting3. Nugget Growth
RP
RE
RD
RP = Resistance PeakRE = Resistance EndRD = Resistance Drop
3
*Constant Current Data
![Page 9: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/9.jpg)
Different materials = Different resistance characteristics
9
Mild/Bare Mild/HDG
AHSS (Boron; Hot Stamped) DP980/EG
3
10 ms to RP ; RD ≅ 40%
25 ms to RP ; RD ≅ 40% 50 ms to RP ; RD ≅ 30%
20 ms to RP ; RD ≅ 20%
*Constant Current Data
![Page 10: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/10.jpg)
Weld current level effects the resistance curve.
10
3
*Constant Current Data
![Page 11: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/11.jpg)
Weld force effects the resistance curve.
11
3
300 lb
450 lb
600 lb
750 lb
900 lb
*Constant Current Data
![Page 12: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/12.jpg)
Weld time effects the resistance curve.
12
3
*Constant Current Data
![Page 13: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/13.jpg)
Pulsation effects the resistance curve.
13
3
*Constant Current Data
3 impulses (80ms @ 9000A , 20ms cool/off)
![Page 14: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/14.jpg)
Different weld locations = Different resistance characteristics
14
3
21 3 4 5 6
Time to RP: 6-30 msRP Value: 260-280 μΩ
*This drives one schedule for each spot.
*Constant Current Data
![Page 15: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/15.jpg)
Expulsion can be detected from the resistance curve, seen as a sharp drop in resistance:
15
3
Too Hot Too LongTooling
*Constant Current Data
![Page 16: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/16.jpg)
Using Constant Current or Volt/Sec Preheat to stabilize the Resistance curves before the start of the adaptive section of the weld.
16
3
![Page 17: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/17.jpg)
17
Later adaptive controls utilize a “reference weld” to enhance the adaptive algorithm.
The reference weld is constant current weld data that is the blueprint for a “good” welding process.
A good reference weld calls for a process that is:◦ Expulsion free◦ Stable◦ Made with proper equipment (dressed tips, adequate power
source, appropriate water cooling etc.)◦ Free of process disturbances◦ Produces quality welds
4
![Page 18: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/18.jpg)
18
Expulsion Free
Stable
Proper Tooling
4
*Constant Current Data
![Page 19: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/19.jpg)
19
0-7 msec: Learned Current
The target current for the beginning of the weld can change based on data analysis.
5
![Page 20: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/20.jpg)
20
7-16 msec: Auto Adjust
Quick adjustment period to correct initial discrepancy.
5
![Page 21: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/21.jpg)
21
16-32 msec: Stable
No current changes to evaluate the process.
5
![Page 22: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/22.jpg)
22
32+ msec: Drive to Peak
Adjust current to achieve a resistance peak, based on the stable period evaluation.
5
![Page 23: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/23.jpg)
23
32+ msec: Realized Peak
A fixed resistance drop must be observed for a realized peak.
5
![Page 24: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/24.jpg)
24
32+ msec: End
Adjust current after peak is realized, and continue until RD and Energy targets are met.
5
![Page 25: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/25.jpg)
25
Time ExtensionIf the target RD and Energy targets are not met, time is extended. If time is extended by
an excessive amount, the learned current is increased for the next weld.
5
![Page 26: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/26.jpg)
26
5
Expulsion Event
Current is increased after an expulsion to add heat & regain the lost nugget material.
![Page 27: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/27.jpg)
Disturbances to the RSW process have major implications on the weld quality.
The ability to detect and adapt to these disturbances can enhance the reliability of RSW.
27
5
Stackup Thickness Increase (+0.3mm)
Stackup Thickness Decrease (-0.5mm)
![Page 28: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/28.jpg)
The decision making algorithm can be adjusted to account for a variety of applications.◦ Type of production – high volume (robot) vs. low volume
(portable gun)◦ Type of material – high strength vs. mild metals; coated vs.
bare metals◦ Constraints – cycle time; secondary current limits
This allows the user to fine-tune the system to make better decisions in every situation.
More flexibility = more complexity◦ This increases the time/knowledge required for proper
setup.
28
5
![Page 29: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/29.jpg)
An adaptive control system requires:◦ Sensors (voltage leads)
◦ Training
◦ Setup
The extra time/cost provide an opportunity to enhance the product quality, especially when a process becomes unstable.
The amount of setup may vary for different applications.◦ In high volume production, stability/repeatability is key.
This is not necessarily true for small scale applications.
29
6
![Page 30: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/30.jpg)
It is crucial to have realistic expectations of an adaptive system.◦ Modern adaptive controls are not perfect.
◦ Poor setup results in improper adaptive decisions.
GSI SLV Duisburg study: ◦ 10 tests comparing adaptive and CC performance using a
variety of materials and disturbances.
◦ These disturbances are common in production environments.
◦ Adaptive control provided noticeable improvement in weld quality.
30
7
![Page 31: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/31.jpg)
31
[4]GSI SLV Duisburg Report: Percent of normal nugget size achieved for 10 disturbances
7
Diameter Compared to Normal
Test Description Step CC (Upper) CC (Lower)Adaptive (Upper)
Adaptive (Lower)
VW01 3-sheet stackupNSSP upper interface 49% 51% 98% 91%
NSSP lower interface 3% 64% 75% 100%
VW02 2-sheet stackupHDG Z100 -> uncoated (+NSSP) 120% - 100% -
HDG Z100 -> Z140 (+NSSP) 42% - 100% -
VW03 Weld with adhesive Adhesive + NSSP 70% - 90% -
VW04 Variation of electrode forceForce 50% 99% - 87% -
Force 150% 75% - 86% -
VW05Shunting effect in a 3-weld
specimen
NS3, 30mm from anchor 67% - 93% -
NS3, 15mm from anchor/weld 2 37% - 88% -
VW06 Functionality of multi pulse weldMulti pulse weld, NSSP upper int. 50% 52% 50% 65%
Multi pulse weld, NSSP lower int. 10% 62% 10% 77%
VW07 Shunting effect + bad fit upNSSP 40mm, +Z material 61% - 99% -
NSSP 25mm, +Z material 52% - 92% -
VW08 Misalignment of parts/electrodes 10° 43% - 20% -
VW09Welding at the edge of the
specimens8mm / 4mm 54% - 58% -
VW11 Electrode life test thin mild steel , HDG550 Welds
Before Undersized
410 Welds Before
Undersized
![Page 32: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/32.jpg)
32
Evaluation Based on Result (Diameter)Test Description Step CC MAX A B C D E F G
VW01 3-sheet stackupNSSP upper interface 1 5 5 3 5 3 3 5 1
NSSP lower interface 1 5 3 5 1 1 1 1 1
VW02 2-sheet stackup
HDG Z100 -> uncoated (+NSSP)
5 5 5 5 5 3 5 5 5
HDG Z100 -> Z140 (+NSSP) 1 5 5 3 3 3 5 1 1
VW03 Weld with adhesive Adhesive + NSSP 1 5 3 3 3 1 3 1 1
VW04 Variation of electrode forceForce 50% 5 5 3 5 3 3 5 5 5
Force 150% 1 5 3 3 3 5 3 1 3
VW05Shunting effect in a 3-weld
specimen
NS3, 30mm from anchor 1 5 5 3 5 3 3 3 1
NS3, 15mm from anchor/weld 2
1 5 3 1 5 1 1 3 1
VW06Functionality of multi pulse
weld
Multi pulse weld, NSSP upper int.
1 5 1 - 1 1 1 3 1
Multi pulse weld, NSSP lower int.
1 5 1 - 1 1 1 1 1
VW07 Shunting effect + bad fit upNSSP 40mm, +Z material 1 5 5 3 5 3 5 3 3
NSSP 25mm, +Z material 1 5 3 3 3 3 5 3 3
VW08Misalignment of parts/electrodes
10° 1 5 1 3 3 5 1 5 5
VW09Welding at the edge of the
specimens8mm / 4mm 1 5 1 1 1 1 1 1 3
VW11 Electrode life test thin mild steel , HDG 3 5 3 3 - - - - -
sum: 26 80 50 44 47 37 43 41 35
[5]GSI SLV Duisburg Report : Comparison of 7 Adaptive Controls for 10 disturbances
7
![Page 33: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/33.jpg)
Advantages Disadvantages
• Real time adjustments provide weld quality enhancements (avoid post-production corrections)
• Automatic response to expulsion events
• Detection and response to unknown disturbances
• Detection and response to expected wear/tear
• Flexible programming for a variety of applications
• Weld data for quality analysis is automatically generated
• Alerts/faults to previously undetected production disturbances are provided
• Additional equipment is needed for resistance feedback (voltage sensors)
• Sensors may require additional maintenance
• Proper setup requires resources (training/knowledge, time, trial parts)
• Difficult to implement during line building stages due to the lack of welded components to establish a reference weld.
33
8
![Page 34: Adaptive Control - Welding Technology Corporation](https://reader031.vdocuments.us/reader031/viewer/2022020623/61f0f3e89b4740047005327f/html5/thumbnails/34.jpg)
[1] WeldCor Supplies Inc. “Resistance Welding.” Weldcor, 2013, www.weldcor.ca/encyclopedia.html?alpha=R&per_page=3.
[2] Ho, C Y, and T K Chu. Electrical Resistivity and Thermal Conductivity of Nine Selected AISI Stainless Steels. 1977, p. 40.
[3] Wang, S. C., and P. S. Wei. “Modeling Dynamic Electrical Resistance During Resistance Spot Welding.” Journal of Heat Transfer, vol. 123, no. 3, June 2001, p. 576., doi:10.1115/1.1370502.
[4]* Schreiber, S. (Ed.). (2016). Test of "intelligent" weld controls for resistance spot welding (VW-Test) (p. 21-59, Rep. No. 2015 661 0759-V).
[5]* Schreiber, S. (Ed.). (2016). Test of "intelligent" weld controls for resistance spot welding (VW-Test) (p. 65, Rep. No. 2015 661 0759-V).
*www.slv-duisburg.de / [email protected]
34