a study of the stress corrosion crack initiation stage in
TRANSCRIPT
![Page 1: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/1.jpg)
Louisiana State UniversityLSU Digital Commons
LSU Historical Dissertations and Theses Graduate School
1995
A Study of the Stress Corrosion Crack InitiationStage in Alpha-Brass.Kun LianLouisiana State University and Agricultural & Mechanical College
Follow this and additional works at: https://digitalcommons.lsu.edu/gradschool_disstheses
This Dissertation is brought to you for free and open access by the Graduate School at LSU Digital Commons. It has been accepted for inclusion inLSU Historical Dissertations and Theses by an authorized administrator of LSU Digital Commons. For more information, please [email protected].
Recommended CitationLian, Kun, "A Study of the Stress Corrosion Crack Initiation Stage in Alpha-Brass." (1995). LSU Historical Dissertations and Theses.6028.https://digitalcommons.lsu.edu/gradschool_disstheses/6028
![Page 2: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/2.jpg)
INFORMATION TO USERS
This manuscript has been reproduced from the microfilm master. UMI films the text directly from the original or copy submitted. Thus, some thesis and dissertation copies are in typewriter face, while others may be from any type of computer printer.
The quality of this reproduction is dependent upon the quality of the copy submitted. Broken or indistinct print, colored or poor quality illustrations and photographs, print bleedthrough, substandard margins, and improper alignment c a n adversely affec t reproduction.
In the unlikely event that the author did not send UMI a complete manuscript and there are missing pages, these will be noted. Also, if unauthorized copyright material had to be removed, a note will indicate the deletion.
Oversize materials (e.g., maps, drawings, charts) are reproduced by sectioning the original, beginning at the upper left-hand comer and continuing from left to right in equal sections with small overlaps. Each original is also photographed in one exposure and is included in reduced form at the back of the book.
Photographs included in the original manuscript have been reproduced xerographically in this copy. Higher quality 6" x 9" black and white photographic prints are available for any photographs or illustrations appearing in this copy for an additional charge. Contact UMI directly to order.
A Bell & Howell Information Company 300 North Z eeb Road. Ann Arbor. Ml 48106-1346 USA
313/761-4700 800/521-0600
![Page 3: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/3.jpg)
![Page 4: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/4.jpg)
A STUDY OF THE STRESS CORROSION CRACK INITIATION STAGE IN ALPHA-BRASS
A Dissertation
Submitted to the Graduate Faculty of the Louisiana State University and
Agricultural and Mechanical College in partial fulfillment of the
requirements for the degree of Doctor of Philosophy
in
The Interdepartmental Program in
Engineering Science
by Kun Lian
B.S., South China Institute of Technology, GuangZhou, China, 1982 M.S., Louisiana State University, 1991
August 1995
![Page 5: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/5.jpg)
UMI Number: 9609102
UMI Microform 9609102 Copyright 1996, by UMI Company. All rights reserved.
This microform edition is protected against unauthorized copying under Title 17, United States Code.
UMI300 North Zeeb Road Ann Arbor, MI 48103
![Page 6: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/6.jpg)
ACKNOWLEDGMENTS
The author would like to extend his sincere gratitude to the following
individuals: Dr. Efstathios I. M eletis, his major Professor, for his advice, tenacious
drive, help, and valuable guidance and suggestions throughout all stages o f this
research. W ithout the help o f Dr. Meletis, this research would not have been possible.
He would also like to express his appreciation and thanks to Dr. Aravamudhan Raman
for his enthusiastic help when the author came to the USA, and during the time he
spent at Louisiana State University. Appreciation and acknowledgm ents also go to Dr.
R obert J. Gale, Dr. Raul E. Macchiavelli, Dr. Su-Seng Pang, Dr. En M a, Dr. R oger R.
M cNeil for their support, time and input.
To his wife Cuihong Tao, he would like to express his deepest felt thanks for
her love, support, understanding , encouragement, and self-sacrifice. His son Guan
Lian, he thanks for his love.
H e wishes to thank his parents and the rest o f his family for their love, and
support.
H e also acknowledges the support by Dr. N. Sarkar and the Louisiana State
University School o f Dentistry, Operative Departm ent, Biomaterials Division for their
support during his study. His thanks also go to W uhan Research Institute o f M aterials
Protection, M inistry o f M achinery Industry, People’s Republic o f China for the support
and understanding.
![Page 7: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/7.jpg)
TABLE OF CONTENTS
A C K N O W L E D G M E N T S ........ ii
L IS T O F T A B L E S ............................................................... vi
L IS T O F F IG U R E S ......... xii
A B S T R A C T ................................................................................................................................ xi
C H A P T E R
I. IN T R O D U C T IO N .................................................................................................... 1
H . O B JE C T IV E S ..............................................................................................................4
H I. R E V IE W O F P R E S E N T U N D E R ST A N D IN G ............................................. 5
A. Historical Background ................................... 5
B. Environm ent-Induced Cracking Phenom ena ............................................ 6
1. Stress Corrosion Cracking ................................................................ 6
2. H ydrogen Embrittlement ................................................................. 10
3. Liquid M etal Embrittlement ........................................................... 13
4. Corrosion-Fatigue ............................................................................. 14
5. W ear-Corrosion Cracking .............................................................. 15
C. Stress Corrosion Cracking in a -B rass ..................................................... 16
D. Present Stress Corrosion Cracking M odels ............................................ 20
1. Dissolution M echanisms ................................................................. 21
2. Film-Induced Cleavage M odel ...................................................... 21
3. Surface Mobility M echanism ........................................................ 22
4. Corrosion-Assisted Cleavage M odel ........................................... 24
5. Corrosion Enhanced Plasticity M odel ........................................ 26
6 . Hydrogen-Induced Cleavage M odel ........................................... 27
![Page 8: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/8.jpg)
E. Corrosion-Deform ation Interactions ........................................................ 28
F. Stress Corrosion Crack Initiation Stage .................................................. 33
1. Deform ation Patterning U nder Environm ental Influence ....... 34
2. Effects o f Electrolyte on Deform ation Patterning .................... 37
IV . E X P E R IM E N T A L P R O C E D U R E S ................................................................ 41
A. M aterial ...... 41
B. Stress Corrosion Cracking Testing ........................................................... 41
C. Corrosion Testing ............... 44
D. Characterization ............................................................................................. 45
1. Scanning Electron M icroscopy ........................ 45
2. Transmission Electron M icroscopy ....................................... 47
3. X-Ray Diffraction ............................................................................. 47
4. Analysis o f Experimental D ata .......................... 48
V. R E SU L T S ........................................................................ 49
A. Evolution o f Deform ation Patterning During SCC .............................. 49
B. Effect o f the SCC Electrolyte .................................................................... 58
C. Dislocation Configuration During TG SCC ....................................... 69
V I. D ISC U SS IO N ..................................................... 75
A. Deform ation Evolution During TGSCC Initiation ............................... 75
1. Environm ent-Induced Surface Plasticity ........... 75
2. Effect o f Anodic Dissolution ......................................................... 77
B. Effect o f Electrolyte Type on TGSCC .................................................... 78
C. Dislocation Arrangement During SCC ............ 80
D. Crack Initiation and Propagation ................ 81
E. Proposed Environm ent-Induced Deform ation
Localization M echanism .............................................................................. 83
1. Vacancy-Dislocation Interaction ............. 87
2. Vacancy Contribution to Crack Propagation ............................ 90
iv
![Page 9: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/9.jpg)
V II. C O N C L U S IO N S .................................................................................................. 96
Vm . SUGGESTED FUTURE RESEARCH ................................................ 98
R E F E R E N C E S ........................................................................................................................ 99
A PPE N D IX E S
A N O M E N C L A T U R E ............................................................................... 110
B H Y D R O S T A T IC STR ESS A N D P L A S T IC Z O N E
C A L C U L A T IO N ........... 113
C P O T E N T IO D Y N A M IC T E S T R E S U L T S O F
a-B R A S S IN D IF F E R E N T E L E C T R O L Y T E S .......................... 115
V IT A .......................................................................................................................................... 119
v
![Page 10: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/10.jpg)
LIST OF TABLES
Table 1. Tafel Slopes and Corrosion Rate o f a -B rass under Stressand Stress Free Conditions........................................................................... 59
Table 2. Strain-to-Initiation, Strain-to-Fracture and Slip Band Spacingo f a -B rass imthe Different Environm ents................................................ 62
Table 3. Calculated Values o f Near-Surface Region Strain.................................. 76
vi
![Page 11: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/11.jpg)
LIST OF FIGURES
F ig u re 1. Schematic plot o f the three stages o f SCC as a function o f stressintensity factor........................................................................................................... 7
F ig u re 2. Schematic anodic polarization curve showing zones o fsusceptibility to stress corrosion cracking.......................................................... 9
F ig u re 3. The relationship betw een the concentration o f copper and(a) the rate o f dissolution and (b) the time-to-failure for Cu-30Zn in 15 M aqueous am m onia" .............................................................................. 19
F ig u re 4. Schematic illustration o f the elements o f the film-inducedcleavage mechanism o f crack propagation........................................................ 23
F ig u re 5. Schematic description o f atomic processes associated withthe surface mobility m odel . 111 ........................................................................... 25
F ig u re 6 . Schematic descriptions o f hydrogen-induced cleavage m odel . 117 ............. 29
F igure 7. Slow strain rate test results on Type 304 stainless steel in boilingM gC k solution . 120 ........................................................................ 31
F ig u re 8 . Effect o f anodic dissolution on creep in pure copper . 121 ............................ 32
F ig u re 9. Relationship betw een plastic strain and dislocation density at thenear-surface region and the interior o f the material in naval brass . 13 ..... 36
F ig u re 10. Schematic diagram o f (a) the experimental specimen and (b) experimental set-up for SCC testing. (All dimensions are in millimeters.)...................................................................................................... 43
F ig u re 11. Schematic illustration o f param eters relating to emergent slipbands on specimen surface................................................................................ 46
![Page 12: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/12.jpg)
Figure 12. Slip band spacing as a function o f plastic strain in a-b rasstested in 5 M N H 4OH solution plus Cu(N03)2............................................. 50
Figure 13. M axim um slip step height as a function o f plastic strain ina-b rass tested in 5 M N H 4OH solution plus Cu(N03)2............................. 51
Figure 14. Scanning electron m icrographs showing a-b rass specim ensurface appearance after straining at lx lO ' 5 s ' 1 in 5 M N H 4 OH solution plus Cu(NC>3 ) 2 (a) zp= 0.002, (b) ep= 0.017,(c) ep = 0 . 1 0 , (d) slip band m orphology in a specim en thatwas strained to fracture in laboratory air, e 0. 75.................................... 53
Figure 15. Scanning electron m icrograph o f an area close to the final stress corrosion fracture surface showing crack initiation patterning (a-b rass tested in 5 M N H 4 O H ).................................................... 55
Figure 16. Scanning electron fractograph showing stress corrosion crack initiation (indicated by arrows) and propagation sites (a-b rass tested in 5 M N H 4 O H )....................... 56
Figure 17. Scanning electron m icrograph showing flat {111} facets producedduring stress corrosion testing (a-brass tested in 5 M N H 4 O H ).............. 57
Figure 18. Scanning electron m icrograph showing (a) surface appearance o f a specim en after 10 m inutes im m ersion in 5 M N H 4OH solution w ith Cu(N03)2, and (b) h igh m agnification o f an area shown in (a)................ 60
Figure 19. Scanning electron m icrograph showing surface appearance o f aspecim en after 10 m inutes im m ersion in 0.1 M CUSO4 solution 61
Figure 20. Fracture surfaces produced by testing (a) in 5 M N H 4OH with C u (N 0 3)2, (b) in 1 M N a N 0 2, (c) in 0.1 M C u S 0 4 and (d) in laboratory a ir ...................................................................................... 64
Figure 21. Slip band spacing developed during SCC testing in thethree electrolytes (solid signs represent crack initiation).......................... 65
![Page 13: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/13.jpg)
F ig u re 22. Typical surface appearance o f slip bands developed in the threeelectrolytes after testing for a total strain o f 0.006 in (a) 5 M N H 4OH with Cu(N03)2, (b) 1 M N a N 0 2 and (c) 0.1 M C u S 0 4 solution 6 6
F ig u re 23. The early stages o f the stress-strain behavior o f a -b rass inthe three electrolytes and in laboratory air.................................................... 67
F ig u re 24. The full w idth ha lf m axim um (FW HM ) m easurem ents o f the {111} peak obtained by X-ray diffraction o f a -b rass specim ens tested in different environm ents....................................................................... 6 8
F ig u re 25. D islocation configuration in an a -b rass SCC specim en(a) a region near the stress corrosion fracture surface showing intensified pile-ups on { 1 1 1 } slip planes and (b) a pure mechanically deform ed region showing a m ore hom ogeneous dislocation distribution................................................. 70
F ig u re 26. A m icrocrack in a -b rass following the < 211> direction(intersection o f the { 1 1 1 } w ith the {0 1 1 } crack plane)............................... 71
F ig u re 27. D islocation configuration in a pure C u SCC specim en (a) a region near the stress corrosion fracture surface showing cellular dislocations w ith traces o f planar slip in the w alls o f the dislocation cells and (b) a pure m echanically deform ed region showing a more hom ogeneous dislocation substructure.......................................................... 73
F ig u re 28. Transm ission electron m icrograph showing dislocation pile-ups associated with dissolution m icrocracks in pure copper. The m icrocrack tip is shown on the upper part o f the m icrograph................. 74
F ig u re 29. Schematic representation o f proposed environm ent-induced dislocation em ission (a) perfect lattice; (b) vacancy generation due to anodic dissolution; (c) generation o f a dislocation and out o f surface displacem ent by one interatomic distance; (d) and (e) form ation o f planar dislocation arrangement; and (f) crack nucleation by opening o f a dislocation pile-up in a slip band ................. 85
F ig u re 30. Schematic representation o f proposed m ultiple dislocationnucleation and fracture surface characteristics produced duringcrack propagation. ............................................................................................. 8 6
![Page 14: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/14.jpg)
F ig u re 31. (a) Stress distribution in front o f a blunted crack in a-brass;(b) Transient divacancy concentration profiles o f stress free(600 s) and stress-assisted (60 s and 600 s) diffusion (C s denotesthe divacancy concentration at the surface.)................................................ 94
F ig u re 32. Potentiodynam ic test results o f a -b rass in 5 M NH 4 0 Hplus Cu(N 03)2 solution...................................................................................... 114
F ig u re 33. Potentiodynam ic test results o f a -b rass in 1 M N a N 0 2 solution 115
F ig u re 34. Potentiodynam ic test results o f a -b rass in 0.1 M C u S 0 4 solution 116
x
![Page 15: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/15.jpg)
ABSTRACT
The objective o f the present work was to provide an insight to the nucleation and
evolution o f deformation patterns occurring during transgranular stress corrosion cracking
(TGSCC) and produce new alternatives for addressing the nature o f the embrittlement
process. Flat, tensile a-brass (72Cu-28Zn) specimens were tested in 5 M NH4OH, 0.1 M
CUSO4 and 1 M N aN 0 2 solutions at a strain rate o f lx lO " 5 s_ 1 . Slip band spacing (SBS)
and slip band heights (SBH) were measured as a function o f strain by conducting
interrupted experiments in the SCC environments and were compared with those developed
during laboratory air experiments. The presence o f the TGSCC-causing environment
during straining was found to promote localized plastic deformation at the near-surface
region, induce strain hardening and more importantly to produce an entirely different
deformation pattern compared to that developed in laboratoiy air. The deformation evolved
in the presence o f the TGSCC electrolytes was highly localized, exhibiting a dense SBS but
coarse SBH. Also, a periodicity was exhibited by the crack initiation process. The amount
o f localized strain developed at the specimen near-surface region prior to nucleation o f
stress corrosion cracks was found to be equivalent to the strain required for ductile fracture
o f the material in air, suggesting the existence o f a fundamental fracture criterion. In view
o f the present observations, an environment-induced deformation localization mechanism is
introduced to explain TGSCC initiation and propagation. The main elements o f the
proposed mechanism are: (i) strain localization due to corrosion instability and periodicity;
(ii) vacancy-induced dislocation emission at the surface region and (iii) vacancy-dislocation
interaction localizing deformation and modifying dislocation arrangement.
![Page 16: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/16.jpg)
CHAPTER I. INTRODUCTION
The problem o f stress corrosion cracking (SCC) has been attracting significant
interest for the last 100 years. A number o f critical engineering com ponents and
structures suffer daily from this and similar types o f environment-induced cracking
(EIC) phenomena with catastrophic consequences in terms o f human life and economic
losses. Fundam ental mechanistic aspects and advances in understanding this
environment-induced embrittlement have been addressed recently . 1 ,2 Even though
several theories have been invoked, there is no broadly accepted mechanism at the
moment to explain these types o f phenomena. The way the environment causes
embrittlement during SCC still remains unresolved and this is an issue o f significant
engineering concern and academic interest.
The m ost significant characteristic o f SCC is that normally ductile alloys
undergo an essentially brittle fracture at relatively low stresses. A specific chemical
environment/material combination and the presence o f a tensile stress are the necessary
requirem ents for SCC to occur. Crack propagation can occur in an intergranular (IG)
and/or transgranular (TG) fashion. Regarding IGSCC, a consensus exists that cracks
initiate at and propagate along grain boundaries according to the film rupture 3 ,4 or the
slip dissolution m odels . 5 In these models, the crack grow s by preferential anodic
dissolution o f the grain boundary region. In contrast, T G cracks generally initiate at
emergent slip bands and propagate on crystallographic planes6 ' 8 by an environmentally-
induced cleavage process, although the way in which the environment induces cleavage
in normally ductile alloys has not been determined yet.
O f particular interest is the case o f TGSCC o f the otherwise ductile face-
centered cubic (FCC) metals and alloys, since they have multiple slip systems and are
1
![Page 17: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/17.jpg)
2
characterized by high dislocation velocities. As has been shown by M eletis and
Hochm an , 6 ' 8 an im portant element o f the underlying TG SCC mechanism is the
ciystallographic nature o f cracking. It has been shown in the above studies that in all
FCC metals and alloys, TG cracks initiate on {111} slip planes but propagate on {0 1 1 }
for non-ferrous metals and on {001} for austenitic stainless steels. All fracture surfaces
consist o f parallel and relatively smooth facets separated by crystallographic or fan
shaped steps. Acoustic emission 9 ,1 0 and electrochemical transien t" studies suggest
that crack propagation is discontinuous, and mating fracture surfaces are matching and
interlocking . 12 Also, crack-arrest markings are usually observed on the fracture
surfaces, and they have been correlated to the discontinuous nature o f crack
propagation.
All the above physical evidence suggests that cracking occurs by a micro
cleavage process. Thus, it is only logical to expect that the deform ation m ode o f the
material would play a key role in the embrittlement process. Previous studies have
shown that the presence o f the SCC environment produces a much higher dislocation
density at the near-surface region , 13 and cracking occurs when a critical value o f
dislocation density is reached . 14 In addition, the fact that cracks initiate on {111} slip
planes, but then change direction and propagate on another plane, suggests that the
param eters involved are contributing to a different extent during crack initiation and
propagation. In the presence o f a growing crack, relatively high stress intensities
prevail and the re-initiation stage is anticipated to be o f short duration and thus difficult
to observe. D ue to their transient character, stress/environment interactions are
expected to have longer lifetime during the very first crack initiation event (occurring
on smooth material surfaces, where a crack has not been formed yet). This provides
the opportunity to study the evolution o f the deform ation process in the presence o f a
SCC environment and to identify possible differences with the deform ation pattern in
![Page 18: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/18.jpg)
the absence o f the cracking-causing environment. Second, it allows the investigation o f
the role o f the plastic deform ation on the TG stress corrosion crack initiation stage, in
an effort to shed m ore light on the fundamental mechanism o f the embrittlement
process. The nature o f the initiation process and its impact on crack propagation may
be fundamental and despite its im portance the crack initiation has attracted very little
attention in the past. A significant role in the SCC initiation process is played also by
the type o f the environment. The fact that in the same metal or alloy certain
environments can cause faster crack initiation compared to other environments that are
m ore corrosive has not been understood yet. The present investigation was conducted
in an effort to provide a better fundamental understanding o f the crack initiation
process during TG SCC and explore its consequences on the crack propagation stage.
![Page 19: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/19.jpg)
CHAPTER II. OBJECTIVES
The specific objectives o f the present research are:
(a) to investigate the nucleation and evolution o f deform ation patterns
occurring during the initiation stage o f TGSCC;
(b) to study the effects o f various TGSCC-causing electrolytes on the
deform ation patterning and correlate them to cracking susceptibility and
the degree o f embrittlement exhibited in the particular electrolyte; and
(c) in view o f the above findings, to produce new insights and new
alternatives for addressing and better understanding the nature o f the
embrittlement process. It is hoped that this investigative effort will
contribute new knowledge to m ore closely defining the operating SCC
mechanism in FCC metals and alloys.
4
![Page 20: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/20.jpg)
CHAPTER III. REVIEW OF PRESENT UNDERSTANDING
A. Historical Background
It is believed that the first docum ented environment-induced cracking is the
“season cracking” o f brass in ammonia-bearing environments in the early tw entieth
century . 1 5 ,1 6 Extensive early w ork on season cracking o f brasses w as carried out by
M oore, Beckinsale, and M allinson . 17 As a result o f their research, an acid m ercurous
nitrate solution w as used to detect susceptibility to season cracking in brasses.
In 1909, another type o f E lC -stress corrosion cracking o f boiler steel was
reported . 18 In 1913, Andrew w as one o f the first to suggest that embrittlem ent caused
by the ingress o f hydrogen into ferric materials, which provided a possible explanation
for SCC in boiler steels . 19 A couple o f years later, Wolff2 0 proposed a fatigue
mechanism accounting for the caustic cracking o f boilers. In 1920, Griffith2 1 first gave
a quantitative relationship betw een the applied energy and crack surface area. By
studying the SCC o f aluminum alloys in 1940, Dix2 2 suggested that chemical
heterogeneity at the grain boundaries was the reason for cracking. In 1947, Keating 23
and Evans2 4 independently suggested that crack propagation occurred by alternating
mechanical and electrochemical stages, in which localized corrosion produced notches
that induced brittle fracture o f a mechanically weakened path. This mechanism requires
a region in the material that is susceptible to corrosion and mechanically weakened,
providing the site for notch o r bulk defect formation.
W ith the developm ent o f new fracture characterization techniques, it was
realized that m icrostructure features such as dislocations may play an im portant role in
the fracture mechanisms. A t the same time, those early hypotheses have been tested
5
![Page 21: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/21.jpg)
and some o f these have gained acceptance. Today, the efforts o f explaining the EIC
are focused on tw o aspects. One is to explain the observed cracking in normally ductile
materials at relatively low stresses with little attendant deformation, and the second is
to determine the role o f specific environments that prom ote such failure.
B. Environment-Induced Cracking Phenomena
EIC can be defined as a brittle failure o r ductility reduction phenom enon in a
particular metal o r alloy when stressed in a given environment. Thus, cracking can
occur only in specific m aterial/environment systems, even though many environments
may be able to produce EIC in a certain material. The various param eters involved in
EIC may include (i) material param eters: composition, crystal structure, m icrostructure,
nature o f grain boundary, deform ation characteristics, and surface condition; (ii)
environmental param eters: nature o f ions, concentration, conductivity, and type o f
phase (i.e. liquid o r gaseous), and (iii) mechanical factors: stress intensity, strain rate,
plane stress/plane strain, loading mode, cyclic frequency, wave shape, etc. Thus, it is
evident that a num ber o f complex physical-mechanical-chemical aspects are involved in
these environm ent-induced fractures.
EIC phenom ena can be classified into the following categories:
I. Stress Corrosion Cracking
SCC can occur in a large number o f material/environment systems. The most
common ones are: brass in ammonia, stainless steel in chloride containing
environments, high strength steels in caustic and nitrate environments, aluminum alloys
in sea water, and Ti alloys in chlorides and methanol. It has been established, that a
certain relationship exists betw een SCC velocity, expressed as: V-da/dt, and the stress
intensity factor Kj, Figure 1. For engineering materials, the rate o f crack grow th in
SCC as a function o f the stress intensity factor at the crack tip shows three regions o f
crack development. In region I, cracks initiate when loading above a threshold value
![Page 22: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/22.jpg)
log
& (
SCC
velo
city
, m
/s)
7
Stage m Rapid SCC Growth /
Stage n Crack Velocity Plateau
Catastrophicfailure
SubcriticalSCCpropagation
Stage I
Timedependent K
SCC
'SCC
1/?Stress Intensity K (MPa* m )
Figure 1. Schematic plot o f the three stages o f SCC as a function o f stress intensity factor.
![Page 23: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/23.jpg)
8
Kiscc and crack velocity is a strong function o f Ki In region II, the crack grow th is
essentially independent o f Ki, indicating the existence o f another controlling param eter
(m ore than likely diffusion controlled). In region III, the crack velocity increases
rapidly with Ki, and unstable crack growth occurs as Ki approaches Kic, the fracture
toughness o f the material. In both stages I and II, the fracture process is influenced
significantly by the environment and generally follows intergranular and/or
transgranular paths. In region III, fracture occurs by a mixture o f environmental and
mechanical cracking (rupture); the proportion o f rupture increases until K i= K ic where
fast fracture occurs.
The electrochemical potential has a critical effect on SCC, especially in
m aterial/environment systems with an active/passive behavior. Figure 2 shows the
potential ranges where SCC occurs in relation to a potentiodynamic anodic polarization
curve for a typical active/passive metal/environment system. Three electrochemical
corrosion reaction zones basically exist in this type o f system: active, passive, and
transpassive or pitting zones. SCC usually occurs in the potential ranges that are at the
beginning or at the end o f the passive region, where the possibility for film breakdow n
exists.
Plastic strain and strain rate also play an important role in stress corrosion
cracking due to the synergistic effects o f the time-dependent corrosion reactions and
microplastic strain. SCC processes require both strain energy and corrosion reactions
in order to initiate and prom ote the crack advancement. Continuous straining exposes
fresh metal surface to the environment and functions as the catalyst to subsequent
environmental reactions. Because the corrosion reactions are chemical reactions and
have a time dependency, a fast strain rate may not allow enough time for corrosion
processes to fulfill their role, thus SCC may not be produced and a ductile fracture is
![Page 24: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/24.jpg)
PO
TE
NT
IAL
9
Pitting
+
A
PassiveCracking zones
Active
lo g C U R R EN T DENSITY
Figure 2. Schematic anodic polarization curve showing zones o f susceptibility to stress corrosion cracking.
![Page 25: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/25.jpg)
10
obtained. A very slow strain rate on the other hand prom otes excessive corrosion
causing crack blunting rather than SCC. A t intermediate strain rates, plastic strain and
corrosion reactions interact critically (synergistically) with each other, and SCC has the
opportunity to occur. It has been shown that slow strain rate testing provides an
excellent way to study these critical corrosion-deform ation interactions.
2. Hydrogen Embrittlement
Even when present in very small amounts, hydrogen can cause severe
embrittlement in many metals, ceramics and intermetallics. Body-centered cubic (BCC)
and hexagonal close-packed (HCP) metals are m ost susceptible to hydrogen
embrittlement (HE), with FCC metals less susceptible . 2 5 The fracture process in HE
can involve cleavage, intergranular, o r ductile fracture depending on the hydrogen
concentration and the stress level . 2 6
The main characteristics o f H E are its strain-rate sensitivity and tem perature
dependence. Unlike m ost EIC processes, HE is enhanced by slow strain rates since
m ore time is provided for hydrogen diffusion. At low and high tem peratures, H E can
be ignored but it is most severe at intermediate tem peratures. H ydrogen can be
introduced in the material in the atomic form (H) in tw o ways. These are,
electrolytically through a discharge reaction (IT+ + e- —> H ) or from a gaseous
atm osphere through molecular dissociation, followed in both cases by H absorption on
a metal surface. D ue to its small size, hydrogen occupies interstitial lattice positions
and diffuses with a high mobility. Because o f the larger interstices and close packing o f
host atom s in FCC and HCP metals than those in BCC metals, usually the mobility o f
hydrogen is less in FCC and H CP metals compared to BCC metals.
The hydrogen transport rates in association with dislocation motion can be
several orders o f magnitude greater than those occurring by diffusion alone . 2 7 In the
presence o f hydrogen, dislocations exhibit higher mobility and velocities and the
![Page 26: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/26.jpg)
opposite effects are observed when hydrogen is removed. The effect o f hydrogen in
stressed metals is to reduce the critical stress required for dislocation motion.
Enhanced dislocation velocities resulting from hydrogen have been observed for screw,
edge, and mixed dislocations and for dislocations that were in tangles, in slip bands, and
far from other dislocations. Similar behaviors have been observed for dislocations in
FCC, BCC, and HCP crystal structures and in alloys as well as in pure m etals . 2 8 ' 3 6
The main proposed H E mechanisms are: (a) lattice decohesion, (b) hydrogen-
dislocation interaction, (c) hydride formation, and (d) hydrogen-enhanced localized
plasticity mechanism.
D ecohesion is one o f the oldest HE mechanisms. In general, decohesion
associates H E with a decrease in the interatomic bond strength. Thus, cleavage
fracture occurs when the applied stress exceeds the lattice “cohesive stress.” The
fracture resulting from HE can be transgranular or intergranular. In IG fracture, the
relevant param eters are the cohesive energy and cohesive force o f the grain boundary,
which are decreased by the presence o f hydrogen as well as the segregation o f many
other solutes. In TG fracture, the fracture surface is usually associated with significant
local plasticity.
For many years, it w as believed that hydrogen dissolved in metals did not
interact significantly with dislocations . 3 7 ,3 8 In the late 60s and early 70s, the opposite
suggestion was made, with strong supporting evidence. Experim ents have shown that
(a) the large values o f the partial molar volume o f hydrogen causes hydrogen-
dislocation interaction in terms o f elastic interactions, (b) internal friction experiments
have shown almost conclusively large hydrogen-dislocation interaction , 3 9 ' 41 and (c) high
resolution autoradiography o f tritium in metals has shown clearly and directly hydrogen
segregation at dislocations . 4 2 ' 4 5 It has been suggested that hydrogen plays an important
![Page 27: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/27.jpg)
12
role in metal embrittlement by interacting with and pinning dislocations, thus permitting
brittle fracture . 4 6 "4 8
A num ber o f metals have dem onstrated HE resulting from stress-induced
form ation o f hydrides or other relatively brittle phases and the subsequent brittle
fracture o f these phases . 4 9 "5 2 The basic requirem ents are that these phases be stabilized
by the presence o f hydrogen and the crack-tip stress field , 5 3 ,5 4 and that the formed
phases be brittle . 55 There are also a num ber o f alloy systems that form “pseudo
hydrides” under cathodic charging. These “pseudo-hydrides” are high-concentration
solid solutions formed in the presence o f a miscibility gap . 5 6 These systems often
exhibit embrittlement in the presence o f this high-concentration, solid solution (or by
the stress-induced formation o f this high-concentration solid solution), even though this
phase is not a true hydride; i.e., it lacks the ordering o f the hydrogen in the interstitial
positions. These stress-induced hydrides remain at the fracture surface and can be
detected in some cases , 5 7 but in other cases, these hydrides must be observed while
under stress . 5 8
Beachem first suggested that hydrogen embrittlement o f steels was in fact
associated with locally enhanced plasticity at the crack tip . 2 6 U nder an applied stress,
hydrogen distribution can be highly non uniform. The high local stress field at the tip
o f a crack reduces the chemical potential o f solute hydrogen , 5 9 and as the result o f
diffusion, the concentration is locally increased. The tip o f the crack is also the most
likely place for hydrogen entry because the plastic deform ation minimizes the surface
barriers. The resistance to dislocation motion, and thus the flow stress, is decreased by
the presence o f hydrogen. So, in the region o f high hydrogen concentration, the flow
stress is decreased and slip occurs at stresses below those required for plastic
deform ation in other parts o f the specimen; i.e., slip localization occurs in the vicinity o f
the crack tip. Thus, the flow stress can be locally reduced, resulting in localized
![Page 28: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/28.jpg)
13
deform ation that leads to highly localized failure by ductile processes, while the total
m acroscopic plastic deform ation remains small.
3. Liquid Metal Embrittlement
Liquid metal embrittlement (LM E) was first reported in the literature in 1874.60
This type o f embrittlement is observed when many ductile metals are coated with a thin
layer o f certain liquid (or low melting point) metals and then are loaded in tension.
Time-to-failure is extremely short, with crack velocities as high as 500 cm/s being
reported for aluminum alloys and brass in the presence o f liquid m ercury . 6 1 ' 6 4 LM E
depends strongly on tem perature. Almost all solid metal/liquid metal couples can
becom e embrittled if a specific tem perature can be reached. LM E usually causes a
cleavage type o f fracture. For FCC metals fracture is mostly IG, while TG fracture
occurs in BCC and HCP metals. Actually, in most situations, a mixture o f IG and TG
fractures co-exists in both FCC and BCC metals.
The m ajor LM E mechanism is chemisorption. It is believed that liquid metal
atom s reduce the cohesive atomic bond strength by chemisorption in the stress
concentration region, allowing fracture to occur at a much low er stress . 6 5 ’6 6 Another
very interesting proposal is the surface charge model. W hen tw o electrically
conducting solids are brought into contact, an electrical double layer is established on
the metal interface, with a potential difference building up at the liquid/solid interface.
This electronic charge layer at the interface would extend only a few atomic diameters
into the solid and could have a strong interaction with dislocations . 6 7 Latanision has
shown that the hardness o f a metal (resistance to the dislocation motion) can be
influenced by the application o f an electrical potential across the surface . 6 8 He
explained this phenomenon by proposing a change in the surface energy by the double
layer potential.
![Page 29: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/29.jpg)
14
4. Corrosion-Fatigue
The simultaneous action o f cyclic stress and environment leading to fracture is
know n as corrosion-fatigue (CF). Usually, materials undergoing cyclic loading in
vacuum at room tem perature show no fatigue limit, and they are not affected by the
cycling frequency (from 1,000 to 12,000 cycles/min.). W hen a corrosive environment
is present, materials show a definite fatigue limit, and they are also affected by the
loading frequency. As a m ajor component o f the EIC phenomena, CF differs from
SCC in several respects. First, it undergoes alternate compressive and tensile stresses.
Second, CF may occur under very low cycle frequency or in the ultrasonic frequency.
Third, the load may be sinusoidal or stochastic. Fourth, the corrosion system may be in
the active or passive state.
It has been shown by a number o f investigators that for pure metals and alloys,
fatigue crack initiation is associated with the production o f intrusions and extrusions by
conventional slip processes. W ithout corrosive environment, the intrusions and
extrusions occur after a saturation o f the cyclic stress occurs . 6 9 ,7 0 During CF processes,
the cyclic loading usually causes cyclic hardening, cyclic softening, or a combination o f
both, provided the stresses exceed the cyclic elastic limit. W hen a corrosive
environment is present, the formation o f microscopic fatigue cracks and crack
propagation can be observed under the stresses below the cyclic fatigue strength in an
inert environment. The morphology o f CF fracture is mainly TG 71 and in general
crystallographic in nature.
Some early w ork on the CF behavior o f mild steel in aqueous sodium chloride
environments suggested that (a) there is a critical corrosion rate below which the
environment does not affect the fatigue crack initiation process; (b) pitting o f the alloy
surface is not necessary to lower the fatigue resistance; (c) passivity enhances fatigue
![Page 30: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/30.jpg)
15
resistance; (d) corrosion rates are progressively higher for higher cyclic stresses, and
(e) the surface deformation characteristics o f the steel are altered by active corrosion.
For stainless steels, corrosive attack w ithout superimposed stress often results
in pitting o f metal surfaces. The pits act as notches and produce a reduction in fatigue
strength. How ever, when a corrosive attack occurs simultaneously with fatigue
loading, a very pronounced reduction in fatigue properties is produced. Traditionally,
CF crack initiation has been associated with pitting7 2 ,7 3 or, with enhanced
electrochemical dissolution resulting from deform ation . 7 4 When films are involved,
rupture o f the protective films by fatigue generated deform ation has also been
implicated in crack initiation . 7 5 ' 7 6
5. Wear-Corrosion Cracking
W ear-corrosion cracking (W CC) is a synergistic phenomenon resulting from
conjoint interactions o f w ear and corrosion in materials. W hen mechanical w ear and
electrochemical processes occur simultaneously, materials deterioration can be
accelerated greatly. It has been suggested by Meletis and Lian7 7 that the wear
corrosion process involves: (a) the disruption and removal o f surface films leading to
exposure o f fresh metal to the environment, and (b) interactions betw een the
environment and elastically or plastically deformed sites at asperities in contact, which
can lead to cracking through wear-corrosion induced embrittlement.
During sliding-wear for example, tension/com pression stress fields are
generated at the vicinity o f the contact. Recent results show that depending on the
properties o f the substrate material and surface film, the combined w ear-corrosion
process can significantly accelerate material degradation due to synergistic effects . 7 8 ,7 9
U nder the activation o f the w ear process, the corrosion potential can be significantly
reduced, and the corrosion current can increase greatly (for example, m ore than tw o
orders o f m agnitude higher for dental amalgams ) . 7 8
![Page 31: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/31.jpg)
16
Sliding-wear/corrosion interactions can also produce subsurface cracking. The
occurrence o f cracking has been observed in our laboratory at LSU in amalgams tested
in chloride solutions . 8 0 W CC also has been reported in ZrCte / w ater system, in which
intergranular WCC was observed under low speed sliding-wear. M eletis81 proposed a
hydrogen-assisted maximum plastic yielding mechanism to account for the observed
embrittlement and cracking in previous studies on w ear-corrosion o f amalgams.
C. Stress Corrosion Cracking in a-Brass
a-b rass is an FCC Cu-Zn alloy with less than 37% Zn. Like m ost o f the FCC
m etals and alloys, a -b rass generally exhibits a ductile behavior and it can undergo
extensive plastic deformation before fracture. How ever, SCC has proved to be one o f
the m ost frequent causes o f failure o f brass equipment in industry. For many years,
brass w as thought to fail only in ammonia environments, but later w ork has shown that
cracking also occurred in non-ammonia environments. These media are sulfate , 8 2 ' 86
acetate, formate, tartrate, hydroxide , 8 7 acidic chloride , 8 8 sodium chlorate , 8 9 m ercurous
nitrate , 9 0 ’9 1 sodium nitrite , 9 2 ’9 3 sodium fluoride , 9 4 and cupric sulfate9 5 solutions.
A lthough many kinds o f solutions can cause SCC in copper-zinc alloys, the a -
brass/aqueous ammonia system has been overwhelmingly studied. In literature, SCC o f
the a-brass/am m onia system has the longest study history, and a large amount o f
available data exists. One m ore advantage o f this system is that it can exhibit both IG
o r T G cracking modes.
Evans suggested that in the a-brass/am m onia system SCC is caused by
ammonium ions which can significantly attack only the grain boundaries or lattice
im perfections . 9 6 Dix has shown that the cracking o f brasses in ammonia solution is
electrochemical in character and that the grain boundary regions are strongly anodic . 9 7
The most common environment used in a -b rass SCC studies is aqueous
ammonia containing dissolved copper, which is the fundamental work done by
![Page 32: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/32.jpg)
M attesson . 9 8 The general corrosion behavior o f a -b rass in such environment is
illustrated in Figure 3(a), which shows the well known relationship betw een corrosion
rate and dissolved copper content . 9 9 ' 101 In order to understand the corrosion behavior
o f a -b rass in the aqueous ammonia solution, the tw o essential redox reactions must be
considered:
Cu = Cu+ + e- ( 1 )
Cu+ = Cu++ + e- (2)
The standard potential for reaction (1) is 520 mV vs N H E, and for (2) is 159 mV vs
NHE. Reaction (2) is slower than (1), so the reaction (2) is controlling the process . 102
The electrochemical reaction is dominated by the form ation o f very stable and soluble
complexes. In moderately concentrated ammonia solution (N H 3 > 1M), cuprous ions
are overwhelmingly present as [Cu(NH 3 )2+] complexes, while cupric ions are present
either as [Cu(NH 3 )4 ++] or [Cu(NH 3 ) 5 + + ] . 103 As the ammonia concentration
increases, the second form complex becomes the main species. So, the reactions (1)
and (2 ) should be rew ritten as:
3Cu + 3N H 3 = Cu+ + Cu(N H 3 )+ + Cu(N H 3 )2+ + 3e" (3)
2Cu+ + 2C u(N H 3 )+ + 2Cu(N H 3 )2+ +9N H 3 = Cu++ + Cu(N H 3 )++ +
C u(N H 3 )2++ + Cu(N H 3 )3++ + Cu(N H 3 )4++ +Cu(NFI3 )5++ + 6 e ' (4)
There are no kinetic data available for the complex reactions. The equilibrium states o f
complex reactions are established very fast, so they do not seem to be the rate
controlling processes. Because the complexes are highly stable, the alkaline ammonia
solution can dissolve fairly large amount o f copper ions before the solubility product
for precipitation o f Cu20 is reached. The solubility product depends on pH and
![Page 33: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/33.jpg)
18
ammonia concentration. By adding reactions (1) and (2), the total corrosion reaction is
obtained:
Cu++ + Cu = 2Cu+ (5)
This corrosion reaction will reach the equilibrium state when the ratio between the
activities o f the uncomplexed species, [Cu++]/[Cu+ ]2, equals the equilibrium constant
K , which is 1.2x10^ at 25°C .104 Because o f the formation o f complexes, the electrode
potential cannot be calculated from the N em st equation. The presence o f zinc in a -
brass does not substantially change the electrochemical behavior because zinc has
relatively fast electrode kinetics in ammonia . 1 0 5 ,1 0 6
Early experimental data showed the strong relationship betw een brass SCC
behavior and copper content in solution. Figure 3(b) shows the results under constant
load at open corrosion po ten tia l." The results indicate that (a) a minimum copper
concentration is required for cracking to initiate, (b) tim e-to-failure is greatly reduced
when dissolved copper concentration increases, and (c) the cracking path changes from
mainly T G to IG. Researchers also like to divide the electrolyte type into tarnishing
and non tarnishing solutions, which is directly related to the copper concentration in the
solutions. It has been established that in tarnishing solutions, IG cracking prevails; and
in non tarnishing solutions, the T G cracking prevails . 107
In non tarnishing solutions, the crack propagation path is dependent on the zinc
content. Brass usually shows IG cracking when the zinc content is less than 18%, and
T G cracking above this value. Zinc content also affects the slip character and the
dislocation structure. One o f the most important observations made in the 1960s and
1970s w as that the TG crack surfaces were cleavage-like in appearance with linear
features resembling fatigue striations. These features are parallel with each other,
![Page 34: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/34.jpg)
TIM
E TO
FA
ILUR
E (s
ec)
RATE
OF
W
EIGH
T LO
SS
(mg/
min
)
19
TarnishFree
0.5
Tarnishing
IntergranularCracking
2 Trans- granular Cracking
COPPER CONTENT (g/I)
F ig u re 3. The relationship between the concentration o f copper and (a) the rate o f dissolution and (b) the tim e-to-failure for Cu-30Zn in 15 M aqueous am m onia."
![Page 35: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/35.jpg)
20
greater than the grain size, perpendicular to the crack propagation direction, and
present atdifferent stress levels . 10 8 All these phenomena indicate that crack
propagation is a discontinuous process, and crack is blunted by plastic deformation
within its arrests. Finally, TG SCC in a -b rass is crystallographic with cracks initiating
on {111} slip planes and propagating on {110} planes. The parallel {110} SCC facets
are separated by crystallographic steps lying on alternating segments o f { 1 1 1 } planes.
This crystallography is com m on to all non-ferrous FCC metals and alloys , 8 and is a
m ajor element o f the TGSCC phenomenology.
D. Present Stress Corrosion Cracking Model
Trem endous efforts have been devoted in the recent years to develop an
understanding o f the SCC mechanism(s). M ost current mechanisms o f SCC are based
on tw o assumptions. One involves the embrittlement o f the metal as a consequence o f
corrosion interaction, and another attributes the SCC to the extremely localized
dissolution processes. All these proposed mechanisms are limited to certain systems or
to some special situations, and still are controversial. At present, there is no
mechanism that can be universally applied to all SCC; however a unified SCC theory
still remains the goal o f most researchers in the field.
A major fundamental aspect o f SCC is the IG or TG m ode o f the cracking path.
In IGSCC, grain boundaries comprise the initiation and propagation sites o f the crack
and a consensus exists that in m ost cases a preferential anodic dissolution mechanism
prevails . 12 On the contrary, as has been shown by M eletis and Hochm an , 8 TG cracking
is crystallographic in nature with the crack initiation and propagation planes not
coinciding. In the latter case, crack propagation is occurring by a microcleavage
process. However, the way in which the environm ent/stress combination induces
cleavage in normally ductile materials has not been established yet.
![Page 36: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/36.jpg)
21
1. Dissolution Mechanisms
The m ost common dissolution mechanism has been used to explain mainly
IGSCC. This mechanism involves tw o elements: (a) preferential and rapid chemical
attack along the plane o f the boundary, which significantly reduces the fracture stress
o f the boundary plane, and (b) pile-up o f dislocations that result in a concentration o f
normal stress across the boundary plane. The unique feature o f this mechanism which
cannot be used on TGSCC is the segregation o f solutes or the precipitation o f discrete
phases that can occur at grain boundaries and that may result in electrochemical
heterogeneity. The driving force for dissolution is related to the potential difference
betw een the matrix and the segregate atoms forming a galvanic cell. Beside the simple
galvanic effects at grain boundaries, it is also possible that film characteristics at grain
boundaries are different with those within the grains. This also can result in preferential
dissolution.
The slip-step dissolution mechanism has been proposed to account for TGSCC.
Slip-steps resulting from plastic deformation emerge at the metal surface. The
protected surface film is disrupted by these slip-steps, exposing the reactive surface to
the environment. Then, the exposed area will be preferentially corroded and become
the crack initiation site. For such a mechanism to operate, the slip-step height should
exceed the thickness o f the surface film.
Another dissolution mechanism that has been introduced by Swann and
Pickering , 1 0 9 is the tunnel model. This model suggests that cracks are initiated at slip
steps by forming arrays o f fine corrosion tunnels which grow in all directions until the
remaining metal ligaments fail by ductile rupture.
2. Film-Induced Cleavage Model
The film-induced cleavage model proposed by Sieradzki and N ew m an 10 is based
on early w ork by Edeleanu and Forty, and emphasizes the role o f dealloyed surface
![Page 37: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/37.jpg)
layers that can initiate microcracking in some materials (e.g. Cu-Zn). As has been
shown by atom ic modelling studies, a brittle crack can initiate in a thin surface film and
obtain a velocity fast enough to penetrate a small distance into the underlying ductile
metal matrix prior to being arrested (Figure 4). The surface film m ust reform at the
crack tip surface before a new burst o f brittle crack grow th is possible. This surface
film could be an oxide, dealloyed layer, or any other kind o f surface layer. The extent
o f the “film-induced cleavage” may be governed by the film-matrix misfit, the strength
o f bonding across the film-matrix interface, the film thickness, film ductility, and the
film structure. It would be reasonable to suppose that hydrogen absorption may also
play an im portant role in such cleavage process. In practice, m ost passive films are
very thin and hydrated, and the dealloyed layers are also unlikely to have sufficient
adhesion to the substrate or have inherent brittleness to sustain cracking. Another
criticism for this mechanism is that it has difficulty in explaining branching o f
propagating cracks.
3. Surface Mobility Mechanism
The surface mobility mechanism, proposed by Galvele , 11 0 suggests that the
advance o f stress corrosion cracks may be modeled by a process that involves surface
diffusion o f species from a stressed cracked tip. Surface diffusivities are significantly
enhanced due to the contam ination o f the metal surfaces from the environment. This
model can be used to explain HE, SCC, LME. The basic principle o f this model is
dem onstrated in Figure 5. An atom at the crack tip is transported by surface diffusion
from its highly stressed location at the crack tip to a new less-stressed site on the crack
walls.
The high stress concentration at the crack tip reduces the free energy o f
vacancy formation, and the equilibrium vacancy concentration at the crack tip is
![Page 38: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/38.jpg)
23
Brittle crack: initiates in brittle film.
P ro p a g a tes in ductile crack tip metal.
Figure 4. Schematic illustration o f the elements o f the film-induced cleavage mechanism o f crack propagation.
![Page 39: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/39.jpg)
24
increased. The surface mobility mechanism assumes that under the action o f the
environment, only the first atomic layers o f the metal are susceptible to measurable
movement. The stress concentration at the tip o f a crack generates a very localized
vacancy deficient region. Every time the stressed lattice at the crack tip captures a
vacancy, the crack propagates by one atomic distance, and a surface depletion o f
vacancies will be created. The diffusion o f those vacancies will be the rate controlling
process, leading to the crack propagation . 111 The main criticisms for this model relate
to relatively low vacancy diffusivities inside the material compared to the observed
SCC velocities and its difficulty in explaining crack branching.
4. C orrosion -A ssisted C leavage M odel
The corrosion-assisted cleavage (CAC) model has been proposed by Flanagan
and Lichter . 1 1 2 ,1 1 3 CAC is based on the interactions between localized anodic
dissolution, localized adsorption and dislocation behavior at the crack tip. It w as shown
that corrosion can enhance local plasticity, which leads to a macroscopically brittle
cracking. This model can be used in both transgranular and intergranular cracking.
In CAC, dislocations generated by mechanical deform ation will pile-up around
the crack tip due to the presence o f Lom er-Cottrell locks near that area. This pile-up
will form an active path for corrosion reactions. This path will be preferentially
corroded away, creating a sharp micro crack, increasing the local stress intensity and
finally initiating a ( 1 10) < 0 0 1 > crack. As the crack grows, the local stress intensity K
drops, and the crack will stop growing when K reaches a critical value. Then, the
corrosion dissolution processes will initiate again, the same process will occur
cyclically, until the material fails. One o f the main deficiencies o f this model is that it
requires the presence o f sessile Lom er-Cottrell locks which are observed only in certain
systems with low stacking fault energy (SFE).
![Page 40: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/40.jpg)
25
S u rfa c e m o b il i ty
C rack g row th
I Metal ion | | Va c a n c yC o n t a m i n a n t
Figure 5. Schematic description o f atom ic processes associated with the surface mobility m odel.1"
![Page 41: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/41.jpg)
26
5. Corrosion Enhanced Plasticity Model
The corrosion enhanced plasticity m odel1 1 4 ,1 1 5 proposed by Magnin, is based on
the principle o f interaction betw een dislocations and corrosion at the crack tip. D ue to
the corrosion interaction with dislocations, there is a large amount o f plastic
deform ation in the micro scale at the crack tip, and the local plasticity is largely
increased. For FCC metals and alloys, this model consists o f the following steps : 116 (a)
depassivation causes a localized anodic dissolution and adsorption on { 1 1 1 } slip planes
at the crack tip; (b) localized dissolution and adsorption result in a stress
concentration, which enhances localized plastic deformation because o f the interaction
among dislocations, adsorption, and localized stresses. The role o f corrosion is
essential but indirect. It enhances the local plasticity at the very crack tip; (c)
dislocations will interact with obstacles, and this will induce the form ation o f pile-ups
where the local stress will increase; (d) if the obstacles are strong enough, local Kic
will be reached. Then an embryo crack will form by a kind o f Stroh mechanism at the
obstacle; (e) the decohesion energy o f { 1 1 1 } microfacets may be decreased by the
adsorption (i.e. hydrogen). The {111} plane will become weaker com pared with other
lattice planes, and cracking will preferentially initiate on this plane. Dislocations are
emitted on asymmetrical planes versus a general crack plane, shielding the new crack
tip. Depending on the crystallographic orientation, this cracking can occur on {111} or
{ 1 0 0 } facets; (f) in the mixed I/II loading mode, this process is expected to lead to
regular changes o f crack planes. A zigzag m icrocracking can occur on {111} and/or
{100} facets. This model has some interesting features but it cannot explain the
formation o f dislocation pile-ups in systems with high SFE such as pure Cu, an element
essential in the model. An advantage o f the corrosion enhanced plasticity model is that
it can be also applied to CF, HE and SCC.
![Page 42: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/42.jpg)
27
6. Hydrogen-Induced Cleavage Model
Hydrogen-assisted cracking is invoked sometimes for BCC materials, but in
conjunction with anodic dissolution has been suggested also for FCC structures. An
interesting proposal has been made recently by Jani et al.,ni based on transmission
electron microscopy (TEM ) studies to characterize the deformation substructure o f 304
stainless steel tested for TG SCC and on earlier w ork by M eletis and H ochm an . 7 The
results showed that the SFE o f the material immediately ahead o f the crack tip is
lowered, with the deform ation m ode at small distances (a few microns) in front o f the
growing crack front being entirely coplanar, while at larger distances hom ogeneous.
Based on these and previous observations o f TGSCC in austenitic stainless steels, a
"hydrogen-induced cleavage" model was proposed with the following sequence o f
events: (a) in the area ahead o f the crack tip, due to the triaxial stress state, the lattice is
expanded and a "hydrogen affected region" (HAR) is formed by the diffusion o f
hydrogen (Figure 6 (a)). (b) Hydrogen in the H A R serves to reduce the SFE within this
volume, therefore restricting cross slip o f dislocations, (c) Planar slip occurs on
intersecting {111} planes that form Lom er-Cottrell locks that are supersessile and lie
on {100} planes, as shown in Figure 6 (b). (d) Since the Lom er-Cottrell barriers are
supersessile, they act as obstacles against glide o f dislocations on the tw o original slip
planes. Therefore, dislocations will pile-up against Lom er-Cottrell barriers, resulting in
extremely high stresses. These stresses will be directed normal to the {100} planes,
and at a critical value, given by the Griffith criterion, the {001} plane ahead o f the
crack will cleave and join up with the pre-existing crack. This is shown schematically
in Figures 6 (c) and 6 (d). (e) After extension, the tip o f the crack will be blunted by
plastic deform ation in front o f it and be arrested. Then the same series o f events will be
repeated.
![Page 43: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/43.jpg)
The new im portant element involved in the "hydrogen-induced cleavage" model
that is supported by the experimental observations is that the corrosion/deform ation
interaction causes a modification in the deform ation mode and the dislocation
configuration at the crack tip. This model requires the presence o f hydrogen for the
m odification o f the deform ation m ode in front o f the crack tip, and indeed, it has been
shown that hydrogen ion form ation and discharge occur readily during TG SCC o f
austenitic steels . 1 1 8 ,1 1 9 How ever, hydrogen involvement has been ruled out from the
TGSCC o f other non-ferrous FCC alloys, such as a-b rass and pure Cu, which basically
exhibit the same cracking phenomenology except that their fracture facets are on {0 1 1 }
planes. Thus, a similar study o f the deformation mode involving these systems would
be o f great interest in establishing the fundamental mechanism o f the embrittlement
process.
E. Corrosion-Deformation Interactions
It is becoming increasingly apparent, that local embrittlement and m icrofracture
can be interpreted in term s o f critical localized corrosion-deform ation interactions
occurring at the near-crack tip region. Both corrosion and deform ation processes can
be greatly enhanced when they occur simultaneously. In the absence o f corrosion,
under slow strain conditions, each element in the metal or alloy undergoes a sequence
o f elastic deform ation, plastic deformation, strain hardening, and finally fracture. In the
presence o f a corrosive environment, the interior elements are unaffected by the
corrosion media, but the exterior elements are attacked (influenced) by the
environment, and becom e "weaker" so the stress required to achieve the same degree
o f strain is significantly reduced. Mom et al.u0 studied the slow strain behavior o f
stainless steels in boiling M gC h and showed that as the strain rate decreases, there is
m ore time for corrosion reactions developing fully, the strain hardening before failure is
gradually diminished by the concurrent effects o f corrosion, but the yield strength is
![Page 44: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/44.jpg)
29
CXACXMOUTH
SUP AND CRACK TIT BIXTNTWO
CSUCXMOUTH
Figure 6. Schematic descriptions o f hydrogen induced cleavage model.
![Page 45: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/45.jpg)
30
unaffected (Figure 7). Because the yielding strength is not affected, the major effect on
the exterior elements by corrosion seems to be a decrease in strain hardening that can
be translated into higher dislocation motion.
Uhlig and co-w orkers 1 2 1 ' 1 2 3 have dem onstrated that anodic surface dissolution
increases the ambient tem perature primary creep rate for both copper and iron. One o f
their examples is shown in Figure 8 , where an applied anodic current clearly increases
the creep rate, which then decreased to the original rate when the applied current was
switched off. Smialowski and Kostanski1 2 4 and Petit and Desjardins125 m ade similar
observations for austenitic stainless steel tested in boiling M gCk solutions. The creep
rate enhancement has been invoked to vacancies produced by the anodic dissolution at
slip steps that migrate into the material and interact with dislocations influencing their
m otion at the near-surface region.
Similar effects have been observed during cyclic straining under a corrosive
environment, with the m orphology o f the C-F fracture surface being different from that
produced in an inert environment. Hahn7 6 ,1 2 6 for example, reported that fatigue surface
shows persistent slip band (PSB) formation early in the 10% cyclic life, while at 90% o f
life cycle the samples show secondary slip bands, which form after significant hardening
has occurred. In the presence o f an anodic corrosion current, the slip bands are
preferentially attacked and the slip distribution at the surface is considerably altered.
On both polycrystals and single crystals o f pure copper, the numbers o f PSB s are
significantly increased and both their heights and breadths are larger.
Besides mechanical effects, corrosion/deform ation interactions can also have
significant effects on corrosion potential and corrosion current, which are the
thermodynamic and kinetic param eters o f the corrosion system, respectively. M eletis et
a l 19 found that amalgam corrosion potential dropped greatly and the corrosion current
increased intensively when sliding-wear was activated on the material's surface
![Page 46: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/46.jpg)
31
O)
2 00
0=glycerine 1=MgQ2, =6 .4 ‘ 1 0 - 5 / s 2=MgC12, =6.4- 10-6 /s 3=MgCl2, =6.4 *10-7/s 4=MgCI2, =6.4 • 10 - 8 / s
100
4 95 6 81 2 3 1070
* • Deformation (mm)
F ig u re 7. Slow strain rate test results on Type 304 stainless steel in boiling M gC h solution . 120
![Page 47: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/47.jpg)
Elo
ngat
ion
32
4 .3 5
4 .3 0
4 .2 5
-P current off
4 .2 0
5
^current on
40 5 0 60 70 8 0 9 0 1 1 0 12 0 100 130 14 0 150
Time, minutes
Figure 8. Effect o f anodic dissolution on creep in pure copper . 121
![Page 48: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/48.jpg)
33
producing tension/com pression stress fields. Jones and co-w orkers 12 7 performed rapid
straining tests and reported a shift in the active potential along with very high anodic
currents. They also noted that a significant increase in anodic current did occur only
when the elastic limit was passed and plastic deform ation had developed. The increase
in the anodic current was attributed to the film rupture by em ergent slip bands.
Parkins 1 2 8 ,1 2 9 studied the interactions in the reversed way. Carbon steel specimens were
stressed and polarized at non-cracking electrochemical potentials in an effort to
suppress the corrosion-deform ation interaction and indeed no cracking was observed.
A considerable volume o f experimental data exists in the literature that can be
interpreted in term s o f corrosion-deform ation interaction that may play a fundamental
role in the embrittlement process. This interaction can mainly be expressed in tw o
forms; as an influence o f the corrosion (environment) process on the dislocation
behavior and as an influence o f plastic deform ation on the electrochemical reactions. A
better understanding o f these interactions would have a lot to offer in shedding more
light on the embrittlement mechanism in an effort to resolve this long standing issue.
F. Stress Corrosion Crack Initiation Stage
The processes preceding crack initiation and propagation should be o f
fundamental importance in understanding the embrittlement mechanism during SCC.
D ue to their transient nature, environm ent-deform ation interactions are expected to
have longer lifetime during the initiation stage, perm itting their easier observation and
study. Thus, the motivation behind the present w ork was first, to study the evolution
o f the deform ation process in the presence o f a SCC environment and identify possible
differences in the absence o f the environment. Second, to assess the role o f the plastic
deform ation patterning on the TGSCC initiation stage, in an effort to shed m ore light
on the crack propagation process.
![Page 49: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/49.jpg)
34
1. Deformation Patterning Under Environmental Influence
There is evidence suggesting that significant differences should be expected in
the deform ation patterns developed in a material that was strained in SCC-free and
SCC-causing environments. For example, K ram er130 reported that a direct correlation
exists betw een the stress at the surface layer and crack propagation rate for com pact
tensile specimens o f Ti-6A1-4V and AISI 4130 steel exposed to H C l-CFbO H and 3
w t% NaCl solution, respectively. It was also shown that different environment/material
combinations will cause different magnitudes o f surface stresses, which is inversely
proportional to the resistance to SCC. A similar observation was reported 131 for
OFHC copper strained in a cupric nitrate-ammonium hydroxide solution that was
known to cause SCC . 1 3 2 The surface layer stress was much higher in the above
solution than in the ammonium hydroxide-copper solution, that causes SCC in brass
but not in copper.
A study o f direct observations o f the dislocation density in SCC specimens was
conducted . 133 The results showed that for 304 stainless steel in a boiling 42 wt%
M gC k solution, the dislocation density in the surface layer increased continuously
under constant stress. On the contrary, samples under the same stress condition but
exposed to an inert atm osphere, showed a slight dislocation density increase at the
beginning, and then remained constant. Yanici134 m easured the dislocation density
change as a function o f distance from the surface o f 304 stainless steel stressed under
constant load in boiling 42 w t% M gC h solution. Initially, the dislocation density in the
surface layer was much higher than that in the interior o f the sample, and both
increased with exposure time. Finally, the tw o dislocation densities became equal and
fracture occurred. However, both dislocation densities were greatly enhanced when
stressing in the SCC environment. Also, both dislocation densities increased very fast
with strain, and cracks occurred when the dislocation density reached a critical value.
![Page 50: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/50.jpg)
K ram er et al.95 studied the relationship betw een dislocation densities and strain
for TG SCC o f naval brass in 0.1 M CuSO t solution, Figure 9. There are several
highlights in their study: (a) the surface layer thickness with a high dislocation density is
about 200 pm and beyond it the dislocation density is constant; (b) cathodically
polarized samples have the same fracture character as the samples stressed in air,
showing a ductile dimple-type fracture; (c) dislocation densities increased linearly with
strain, and the density on the surface is always higher than that in the interior; (d) the
surface layer dislocation density curves do not pass through the origin except for the
interior dislocation density stressed in air. This indicates that once the material is
exposed to the environment, the environm ent-deform ation interaction results in a
sudden dislocation density increase; (e) for naval brass in 0.1 M C uS04 solution, SCC
11 2occurred w hen the surface layer dislocation density reached a value o f 4.5x10 cm' .
This is also the value reached in plastic fracture o f specimens strained in air and under
cathodic polarization; (f) the dislocation density on CF fracture surfaces also has the
same value as that obtained from specimens fractured in a SCC environm ent and in air.
An interesting finding in this report is that by removing periodically the surface layer o f
the SCC specimens, the time before cracking initiation w as extended and the total
strain could reach 30%. When cracking finally occurred, the surface and interior
dislocation densities reached the same values as in the SCC samples. This shows that
crack initiation has a close relationship with the surface layer strain and dislocation
density.
The crystallographic nature o f cracking is another im portant clue to
understanding the initiation and propagation mechanisms o f SCC, especially o f
TGSCC. This topic was reviewed by M eletis7 ,8 for FCC metals and alloys. The results
showed that for TGSCC in austenitic stainless steels, {0 0 1 } is the predom inant
cracking plane with some secondary cracking on {110} planes. The crack propagation
![Page 51: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/51.jpg)
36
7
O l * I ' I I 1 1 I I0 4 8 12 16 20 24
€ %28 32
Sym bol Sym bol Environment Potentialfor data for data (m V (S C E ))obtained obtainedat the in thesurface interior
o , *, A irA , - — A , - - ~ 0.1 M C u S 0 4
0 , ------- « , -------- 0 .1 M C u S 0 4 + 5400 fi 0 .1 M C u S 0 4 + 3 0 0V T 0.1 M C u S 0 4 - 5 4 0
F ig u re 9. Relationship between plastic strain and dislocation density at thenear-surface region and the interior o f the material in naval brass.13
![Page 52: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/52.jpg)
37
process has been shown to be discontinuous1 2 ,1 3 5 and fractographic features on mating
fracture surfaces are found to be matching and interlocking . 8 For non-ferrous metals or
alloys, such as Cu, Cu3 Au, a-brass, etc., the crack initiates on {111} planes, but
propagation occurs on {110} planes rather than lying along {111} slip planes. Lichter,
et al.,m found that the TG fracture surfaces generated during SCC o f ordered and
disordered CU3 -AU are essentially identical to those that form during TG cracking o f a -
brass in ammonia. The fractures appeared to occur by discontinuous cleavage with
{ 1 1 0 }-type cleavage steps, and crack-arrest marks perpendicular to the direction o f
crack grow th w ere present.
2. Effects of Electrolyte on Deformation Patterning
It is generally accepted that SCC occurs easily in certain specific environments.
The chemistry o f the electrolyte in which the material undergoes SCC should be a key
factor to understand the mechanism o f the SCC phenomena. Unfortunately, very little
attention has been given to this very important issue. An understanding o f the effects
o f the electrolyte type on the SCC process can contribute significantly to the
establishment o f the SCC mechanism, but also aid in the practical prevention or
inhibition o f SCC in service.
Althof4 3 7 made an important contribution to understanding the role o f the
ammonia environment in SCC o f a-b rass back in 1944. He dem onstrated that cracking
did not occur until the testing solution turned blue and that the stress corrosion life was
remarkably reduced when the test solutions were pre-saturated with copper ions. It is
known that in aqueous ammonia solutions, copper exists as cupric complex ions o f the
type Cu(NH 3 )n2+, the number o f ammonia ligands, n, varying from 1 to 5 depending on
the ammonia concentration o f the solution . 138 The presence o f these complex ions gives
rise to the blue color o f the solution. Another important variable o f am m onia/a-brass is
the concentration o f ammonia. M ost studies in the past were performed in 15 N
![Page 53: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/53.jpg)
38
aqueous N H 3 , but Pugh et a / .139 showed that experiments conducted in 15 N and 1 N
solutions pre-concentrated with copper produced rapid cracking in both solutions. The
spectrophotom etric studies illustrated that the predominant complex species were
Cu(NH3)52+ and Cu(NH3)42', respectively. It seems that for SCC to occur in the
ammonia/ot-brass system, the concentration o f ammonia can be varied in certain range
as long as the cupric complex ions can be formed.
The effects o f varying the complex ion concentration on the SCC behavior o f
70-30 brass tested in 15 N aqueous ammonia w ere extensively studied.99 Figure 3
illustrates the relationship betw een time-to-failure and the rate o f weight loss for
specimens tested under constant load and copper content o f the solution, which was
directly proportional to the concentration o f Cu(NH3)52+ ions. The tim e-to-failure
decreased w ith increasing concentration o f copper. Also, a well defined inflection
occurred at a critical concentration. Specimens tested in solutions o f copper content
exceeding the critical value were coated with the characteristic black oxide coating
commonly term ed the tarnish, while the specimens tested in solutions o f lower
concentrations w ere apparently free from this coating. The relationship betw een rate o f
weight loss and copper content o f the solution also exhibited a maximum at this critical
concentration.
Thus, it is evident that the electrolyte chemistry is an im portant param eter in
determining the SCC behavior o f a system. Num erous experimental studies and
modeling efforts have been conducted in the past and the present w ork will not make
any attem pt in that direction. Having an overall look o f previous observations on
environm ent/deform ation interactions, it seems that the environment exercises a critical
effect on deform ation and dislocation behavior in particular. It is interesting to note
that this effect is present even in environments that may cause minimal o r no corrosion
at all in the material. Apparently, some type o f interaction may exist betw een the
![Page 54: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/54.jpg)
39
surface layer o f the material as has been modified by the presence o f the electrolyte and
the dislocations present in the near-surface region. A possibility is that an important
effect on aqueous environment/material systems may be exercised by the double layer
structure betw een the electrolyte and the m aterial’s surface (usually metal surface).
Different electrolyte/material combinations will form different double layer structures
and different tendencies to corrosion reactions, which are reflected on the different
corrosion potentials for different material/electrolyte combinations. It has been
discussed before that the SCC phenomena have intrinsic relation with dislocations in
the material and that there is a much higher dislocation density on the crack tip and the
specim en’s surface when SCC occurred.
For clean metallic material surfaces (under vacuum), it was suggested by
Fleischer140 that dislocation nucleation at the surface will be different from that in the
bulk material because the lattice spacing in the surface layer w as different from the bulk
spacing, which is called “relaxation” . This difference will inhibit dislocation nucleation
on the surface layer. Low-energy-electron-diffraction (LEED ) studies141,142 have
shown that “relaxation” o f the lattice occurs in the atomic spacing for several atomic
layers ju st beneath clean surfaces, where the atomic spacing between the first and
second layers is generally contracted compared with the bulk. Occasionally, the surface
lattice even has a different structure from the bulk, which is term ed “reconstruction” .
B oth relaxation and reconstruction are expected to change the dislocation nucleation
and m otion in the near-surface layer o f the material.
Surface relaxation and reconstruction essentially happen because surface atoms
have few er neighbors than those in the bulk. W hen a metal comes in contact with an
electrolyte and the double layer structure is established on the m etal’s surface,
especially in the form o f complex o f the metal ions, the atomic forces acting on the
atom s in the near-surface layer will change significantly. Thus, it should not be
![Page 55: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/55.jpg)
surprising that dislocation nucleation, configuration, and motion may be significantly
influenced by the double layer. This expectation can be relating to the effects o f the
double layer on modifying the image force. A reduction o f the image force by the
particular double layer (producing a low modulus surface layer) can significantly
enhance dislocation motion to the surface and cause localization o f strain. Another
possibility relates to the interaction o f the electrical charges from the double layer with
dislocations and vacancies in the near-surface region o f the material that can also
change dislocation nucleation, configuration, and movement, that is o f primary
im portance to the SCC mechanism.
![Page 56: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/56.jpg)
CHAPTER IV. EXPERIMENTAL PROCEDURES
A. Material
The tes t m aterial selected in the present study w as a -b ra s s due to the large
am ount o f available da ta and extensive previous studies. Tensile specim ens w ere
p repared from a cold rolled a -b ra ss sheet w ith 10 mm gauge length, 5 mm width,
and 0.5 mm thickness, F igure 10 (a). The nom inal com position o f the m aterial w as
72 w t% C u and 28 w t% Zn. Specim ens w ere first stre tched to about 3% and then,
encapsulated in quartz tubes under vacuum and recrystallized by heating at 900° C
fo r 48 hrs to p roduce a final grain size o f about 1 mm. All specim ens w ere ground,
fine polished, and electropolished in 3:1, m ethanol/conc. H N 03 a t -3 0 ° C and 8V
for about 2 min. in o rder to ge t m irror-like, stress-free surfaces.
In addition, sm ooth, cylindrical, single crystal specim ens o f a -b ra s s and
pure copper (99 .999% purity ) w ere used fo r the dislocation configuration studies.
The rationale behind selecting pure Cu in addition to a -b ra ss is th a t Cu has a
relatively high SFE com pared to a -b ra ss and an additional insight can be gained.
Single crystal specim ens w ere used in o rder to avoid com plexities arising from
grain boundary effects easing TEM observations. The gauge lengths o f these
specim ens w ere 25 mm and specim ens w ere 5 mm in diam eter. The single crystals
w ere g row n using the B ridgm an technique. They w ere all e lectropo lished as the
flat a -b ra s s tensile specim ens.
B. Stress Corrosion Cracking Testing
SCC testing was conducted using the slow strain rate technique to study the
evolution o f the deform ation patterning in the a-brass/5 M NHUOH system. The effect
o f the electrolyte type on the deform ation patterning was investigated by conducting
41
![Page 57: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/57.jpg)
42
slow strain ra te tes ts in th ree different electro lytes and determ ining the deform ation
characteristics on the surface o f strained specimens. In addition, electrolyte effects
w ere studied by conducting straining experiments and subsequently determining near
surface dislocation densities as described later. The three electrolytes selected for the
present w ork were: 5 M N H 4 OH with 8 g/1 Cu added as Cu(N03)2, 0.1 M CuSO t, and
1 M NaNCte solutions. The rationale behind this selection is that, while a -b rass shows
different corrosion behavior in these electrolytes, they all have been found to cause
TG SCC in this material.
The SCC testing included the following slow strain rate experiments: (i) testing
in the particular electrolyte to obtain the strain-to-fracture under SCC conditions, ascc
and (ii) testing for various levels o f straining in the SCC solution to allow determination
o f the deform ation characteristics as a function o f strain. Similar control experiments
w ere conducted in laboratory air and served as standards for comparison. Three repeat
tests w ere conducted for each testing condition.
The slow strain rate tests were carried out using an electrically driven
M echanical Testing System (CORTEST Model 6100). A strain rate o f lx lO '5 s"1 was
applied. It has been established previously by Kramer,95 and by the author, that this
strain rate is suitable for the SCC study o f a-brass. The specimens w ere attached to a
pair o f fiberglass grips in order to allow electrochemical testing during straining. A
plastic cup was positioned and sealed around the gauge length o f the specimens and
filled with the electrolyte. Finally, a salt bridge that was connected to a reference
saturated calomel electrode (SCE) and a pair o f graphite counter electrodes were
positioned in the cell and connected to the electrochemical testing system (EG& G
Potentiostat M odel 273 with M 342C software), Figure 10 (b).
Slow strain rate experiments were also conducted on a-b rass and pure copper
single crystals to study the dislocation substructure during TGSCC. Cylindrical single
![Page 58: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/58.jpg)
II
h
c E
vve
Figure lo o ,
Sel-«P A r sc c ° f(a; "><> ®per^ testing ( a i. , .p rimental cnQ •(■AH dimensions P omen and Ch\"S'0nsare i„ mi„im ™ W eXperimen(a;
![Page 59: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/59.jpg)
44
crystal a -b rass and pure copper specimens were strained to fracture in 5 M NH4OH
and 1 M N aN ( > 2 aqueous solution, respectively. A strain rate o f lxlO "5 s '1 was also
used in these experiments. Part o f the gauge length o f these specimens was covered
with an insulating lacquer to avoid contact with the electrolyte and to restrict
environmental action in a certain section o f the gauge length. This allowed preparation
o f TEM foils from areas w ith and w ithout environmental interaction as described in the
next section.
C. Corrosion Testing
The effect o f the electrolyte type on SCC was studied by performing
electrochemical tests in strained and unstrained specimens. First, the corrosion
behavior o f a -b rass in the three different electrolytes was studied by carrying out
anodic polarization tests. Dissolution rates o f unstrained and strained a-b rass
specimens w ere determined by conducting polarization resistance experiments. The
Tafel slope values needed to calculate the dissolution rates were obtained from the
anodic polarization tests o f unstrained specimens in all three electrolytes. The
polarization resistance tests during straining were conducted to determine the effect o f
mechanical deform ation on the corrosion rate. This m ethod was used for estimating
the corrosion rate in order to minimize applied potential disturbances with corrosion
processes especially for stressed specimens. Second, pure immersion tests w ere also
conducted o f unstressed a -b rass in all three electrolytes to investigate surface
characteristics and possible patterning o f the corrosion process.
All corrosion experiments were conducted by using an EG & G Corrosion
M easurem ent System (M odel 273 with M 342C Corrosion Software). For all
polarization experiments, the specimens were exposed to the solution for 10 min. prior
to testing. The anodic polarization scans started at about 300 mV below the corrosion
potential, Ecorr, and progressed up to 300 mV above Ecorr at a rate o f 1 mV/s. The
polarization resistance tests w ere conducted by polarizing at ±20 mV from the open
![Page 60: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/60.jpg)
45
circuit corrosion potential at a scan rate o f 0.3 mV/s. The tensile specimens used for
polarization resistance tests during straining were masked by using an insulating lacquer
leaving only a certain area o f the gauge length exposed to the electrolyte. Five
polarization tests with reproducible results were performed during straining in each
electrolyte, (Table 1) starting before the elastic limit o f the material and progressing up
to a total strain o f about a = 6%.
Pure immersion tests w ere conducted by placing annealed a -b rass specimens
approximately lx l cm^ in area and about 0.5 mm thickness in the three electrolytes.
The duration o f these tests w as 10 minutes. After testing, the specimens w ere rinsed in
distilled water, dried by com pressed air and immediately examined using scanning
electron m icroscopy (SEM ).
D. Characterization
1. Scanning Electron Microscopy
Scanning electron m icroscopy (ISI 60A and HITACHI S2700) was used in the
present study to characterize the evolution o f deform ation patterning under the
environmental influence. The development o f the deform ation patterning was
characterized by m easuring the slip band spacing (SBS), slip band height (SBH ) and
slip band length (SBL) at various strain levels. Figure 11 schematically illustrates these
param eters in relation to the specimen surface. Slip band height refers to the thickness
(or height) o f the slip band and is directly proportional to the number o f slip planes
involved in the slip band. Crack initiation spacing (CIS), which is the distance between
fine cracks was also used to describe the deformation pattern. D ue to the
polycrystalline nature o f the specimens, measurements were taken in at least three
different grains showing the largest amount o f plastic deformation. Also, in the
interrupted deform ation experiments, markings were lightly scribed on the specimen
surfaces to allow identification o f the same locations for measurements.
![Page 61: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/61.jpg)
slip direction
slip b a n d length
S S S 'v$Cq /} O f
ra.ers
Qtj,
er.
!Pb,Of}
![Page 62: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/62.jpg)
47
SEM was also used to conduct fractographic studies after SCC testing and
examine specimen surfaces after immersion testing in the three different electrolytes.
2. Transmission Electron Microscopy
An analytical TEM (Jeol 100c) was used to characterize the deform ation
substructure in the cylindrical single crystal SCC samples. Thin discs o f the tested
specimens were obtained from the SCC fracture surfaces and sites protected by the
insulating coating (no environmental influence). Electron transparent thin foils were
prepared by electropolishing in a solution containing 75% methanol and 25% H N 0 3 at
a tem perature o f -30° C and voltage o f 10 V. Electropolishing was carried out on a
Tenupol-2 unit (Struers) using both the single-jet and tw o-jet technique. TEM was
performed at 100 keV and electron diffraction was used to identify crystallographic
orientations in the foils.
3. X-Ray Diffraction
The dislocation densities in the near-surface layers o f the a -b rass specimens
produced by straining in the different electrolytes w ere studied by X-ray diffraction
(XRD) techniques. The a -b rass specimens used in the XRD study had an average
grain size o f about 70 pm. These specimens were produced from the originally
stretched specimens (3% ) by annealing at 550 °C for 1 hr. The purpose o f using
sm aller grain size specim ens in the X RD study w as to increase the accu racy o f
th e measurement and reduce the variation among different specimens. XRD in the
present study was conducted by using a Rigacu D-M ax 2B X-ray diffractometer, which
w as equipped with a diffraction beam graphite monochrometer. Copper Ka radiation
w as used with a wavelength o f 1.542 A. An acceleration voltage o f 35 keV and a
current o f 25 mA were used. The full-width half maximum (FW HM ) o f the {111}
diffraction peak was m easured for annealed specimens and specimens strained in air
and in the various electrolytes. The broadening o f FW HM was taken as a measure o f
![Page 63: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/63.jpg)
48
plastic deformation (dislocation density) in the near-surface region o f the specimens to
allow comparison o f the effect o f the electrolyte type on dislocation density.
4. Analysis of Experimental Data
The effects o f electrolyte type on FW HM values were studied by using the
analysis o f variance (ANOVA) m ethod. Paired comparisons w ere conducted to study
the specific differences. The effects o f the electrolyte type on the corrosion rate in the
stress free condition were analyzed by conducting tw o tails heteroscedastic T test. The
effects o f stress on the corrosion rate were investigated by applying general linear
models procedure (GLM ) with the data transfer. The data transform ation was
performed by taking unstressed data as unity. All the analyses w ere conducted by using
statistical analysis system (SAS) program with a 0.95 confidence coefficient.
![Page 64: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/64.jpg)
CHAPTER V. RESULTS
A. Evolution of Deformation Patterning During SCC
Figure 12 shows the variation o f SBS as a function o f plastic strain for
experiments conducted at the same strain rate in laboratory air and in the 5M N H 4 OH
solution. As would have been expected, the SBS for the specimens tested in laboratory
air is larger initially and gradually decreases with strain since the slip band density is
proportional to the magnitude o f the plastic strain. These specimens w ere quite ductile
and showed a strain-to-failure o f about s j = 0.75. The results also show that a t the
initial stages o f deformation, there is a significant difference betw een prominent
(coarse) SBS and average SBS, but eventually this difference is diminished. In
contrast, slip during SCC testing exhibits an entirely different pattern. The SBS for
these experiments is very fine at the initial stages o f the deform ation process and
increases with strain reaching a plateau value o f about 14 pm at fracture. The
approxim ate strain-to-failure for the stress corrosion specimens was about escc = 10%.
SEM examination showed that crack initiation had ju st occurred in the specimens that
w ere strained at a plastic strain o f 8p= 0.002. Also, a strain hardening effect was
observed in the stress/strain curves o f the SCC experiments compared to the
experiments in air.
Figure 13 shows the variation o f the maximum SBH as a function o f plastic
strain. The slip band heights for straining in laboratory air w ere too small (in the order
o f nm) to be measured precisely and w ere therefore theoretically calculated by using a
model developed by Eshelby et al.143 This model has been previously applied for ex-
brass by Yu et al.144 and showed very reasonable agreement with experimental values
obtained by using optical interferometry. Based on the above model, the SSH (h) is the
49
![Page 65: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/65.jpg)
Slip
B
and
Sp
ac
ing
50
20 n a-brass L a b o ra to ry Air □ Average SBS ■ Coarse SBS
SCC E nv ironm en t O C oarse SBS
- 5
gra in
ED
0 -
6 -
4 -
250 5 10 15 20P l a s t i c S t r a i n , %
F ig u re 12. Slip band spacing as a function o f plastic strain in a -b rass tested in 5 M N H 4OH solution plus Cu(N 03)2.
![Page 66: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/66.jpg)
Slip
St
ep
Hei
gh
t,
51
Ot—brass □ L a b o ra to ry Air O SCC E n v iro n m e n t
- 5
1 0 -
- 0.8
0.6
6 -
- 0.4
4 -
- 0.2
0.0
P l a s t i c S t r a i n , %
Figure 13. M aximum slip step height as a function o f plastic strain in a -b ra ss tested in 5 M N H 4OH solution plus Cu(N 03)2.
Slip
St
ep
Hei
gh
t,
![Page 67: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/67.jpg)
52
result o f a pile-up o f n screw dislocations with Burgers vector b gliding out o f the free
surface:
G M ' (6)
where <p is an orientation factor (between 0.71 and 0.75), G is the shear modulus
(about 37 GN/m2 for a-b rass), M = 2.2 is a Taylor average orientation coefficient for
shear in polycrystalline material, k is the slope in the Hall-Petch relationship and I is the
average grain diameter (1 mm). Arm strong et al.145 showed that for 70Cu-30Zn k
changes very little (from 0.34 M N/m 3/2 at yield to 0.374 M N/m 3/2 at 0.2 strain)
producing a relatively insensitive variation o f the SSH with strain in laboratory air. The
SSHs developed during the SCC experiments were substantially larger (by a factor o f
about 25) compared to the step heights in air. Thus, the presence o f the SCC
electrolyte was found to result in environment-induced slip, prom oting deformation
localization in the form o f finely spaced coarse slip bands.
Figures 14 (a)-(c) are scanning electron micrographs from surfaces o f
specimens that were strained at £p = 0.002, 0.017 and 0.10, respectively, in the stress
corrosion electrolyte (5 M NFUOH). It is evident from these micrographs, that crack
initiation occurs along {111} traces at the very early stages o f straining. Such TGSCC
along emergent slip bands on the surface is typical for FCC materials. Also, a fine SBS
develops initially in these experiments with coarse SBH and slip band length. As strain
increases, the deformation becom es coarser in all respects, with increasing SBS, SSH
and SBL. Figure 14 (d) presents a typical slip band m orphology on a specimen surface
that was strained to fracture in air {ej « 0.75). The slip band spacing in specimens
![Page 68: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/68.jpg)
Figure 14. Scanning electron m icrographs showing a-brass specimen surfaceappearance after straining at lx lO '5 s '1 in 5 M N H 4 OH solution plus Cu(NCb ) 2 (a) £p= 0.002, (b) &p- 0.017, (c) sp = 0.10, (d) slip band m orphology in a specimen that was strained to fracture in laboratory air, £/■« 0.75.
![Page 69: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/69.jpg)
54
strained to failure in air was very similar to that m easured in specimens strained at 8p
0.002 in the N H 4 O H environment {d « 1.5 pm, Fig. 12). Nevertheless that morphology
w as quite different with very shallow slip band heights as predicted by Equation (6).
Figure 15 presents an area close to the final fracture surface in a SCC specimen.
Besides the presence o f coarse slip at the near-surface region, the m icrograph shows a
series o f regularly-spaced micro- and m acro-cracks that were initiated along the traces
o f the {111} primary slip planes. M ore importantly, it was observed in the present
w ork that a periodicity exists in the occurrence o f crack initiation (between 6-10 pm,
Fig. 14). A relation also exists betw een SBS and CIS. For example, specimens that
w ere strained at ep - 0.002 exhibited a CIS o f about 6 pm and a SBS o f about 2 pm,
showing that a crack initiation event was activated for every three slip bands. The
transition from initiation to propagation was evident on the SCC specimens, Figure 16,
with the crack initiation site extending for about 50-80 pm. Also, the crack initiation
facets w ere highly crystallographic and featureless as shown in Figure 17.
The potential measurements showed that the corrosion potential o f the
specimens stabilized at about -450 mV (SCE) prior to straining and decreased by about
20-50 mV during straining. The anodic and cathodic Tafel slopes determined from the
anodic polarization experiments were pa = 383±45 mV and fic = 387±32 mV,
respectively. The anodic dissolution rates determined from the polarization
experiments, w ere found to be 5.9 ±0.6 mA/cm2 and 6.7 ±0.05 mA/cm2 for unstressed
and stressed specimens, respectively. It is interesting to note that no statistical
difference was determined in the corrosion rates between elastically (just before the
elastic limit) and plastically stressed specimens. This behavior is in agreement with
earlier slow strain rate results, where strain induced dealloying o f Cu-Zn alloys was
evidenced even with final loads appreciably lower than the 0.1 pet offset yield stress.146
![Page 70: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/70.jpg)
55
F ig u re 15. Scanning electron m icrograph o f an area close to the final stress corrosion fracture surface showing crack initiation patterning (a-b rass tested in 5 M N H 4OH).
![Page 71: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/71.jpg)
56
■ . '■' ■ ■' v*'- i Vu a ■ -■--*,* ■# <**>&'*':■■?■**:•?£. *• ’-• -,
Figure 16. Scanning electron fractograph showing stress corrosion crack y initiation (indicated by arrows) and propagation sites (a-b rass tested in 5 M N H 4OH).
![Page 72: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/72.jpg)
57
F ig u re 17. Scanning electron m icrograph showing flat {111} facets produced during stress corrosion testing (a-b rass tested in 5 M N H 4 OH).
![Page 73: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/73.jpg)
58
B. Effect of the SCC Electrolyte
Table 1 presents the corrosion rates o f stressed and unstressed brass in the three
different electrolytes. The results showed that the corrosion rate o f a-b rass is
significantly different in the three electrolytes. The 5 M N H 4 OH solution was the most
aggressive environment exhibiting the highest corrosion rate, whereas 1 M NaNCh
showed the lowest corrosion rate. In all cases the application o f stress was found to
increase the corrosion rate significantly. The GLM analysis also showed that the
relative increase in the corrosion rate due to stress was similar for N H 4 OH and CuSCh.
It is interesting to note that the greatest increase (almost one order o f magnitude) was
observed for 1 M NaNCh which exhibited the lowest corrosion rate in the experiments
w ithout the application o f stress. Consistent with the above results, the immersion tests
showed that significant corrosion had taken place in the N H 4 OH and CuS04 solutions,
but no evidence o f any attack was found for the NaNCh solution. Observations o f
specimens that w ere exposed in the form er tw o solutions indicated that corrosion in
N H 4 O H exhibited preferential dissolution resulting in a m orphological pattern with
evidence o f periodicity, resembling that o f slip bands developed under stress, Figures
18 (a) and (b). A rather random, corrosion attack was observed on surfaces o f
specimens that were exposed in the CuSC>4 solution, Figure 19. The anodic
polarization curves (Appendix C) showed that a -b rass passivated only in the 1 M
NaNCh solution. Thus, the low corrosion current in the absence o f stress in the above
electrolyte was m ore than likely due to passive film formation. Upon application o f
stress, the film was ruptured exposing fresh metal surface to the electrolyte, thus
increasing the corrosion rate.
Table 2 presents the total strain to crack initiation, total strain-to-fracture and
the SBS at fracture for all three SCC electrolytes and for the experiments in laboratory
air. T otal strain rather than plastic strain w as used due to possible environm ental
![Page 74: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/74.jpg)
59T ab le 1. Tafel Slopes and Corrosion Rate o f a-B rass under Stress and Stress Free
Conditions
SolutionsTafel slope
Pc(mV) Pa(mV)
2C orrosion C urren t(p .A /cm )
Stress free U nder stress
0.1 M CuS04 350±9 276±5 1535±142 1796±61
1 M NaN02 469±67 56±2 7±1 67±1
5 M NH^/Cu** 387132 383±45 5979±592 6777155
Values are based on five measurements.
![Page 75: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/75.jpg)
F ig u re 18. Scanning electron m icrograph showing (a) surface appearance o f aspecimen after 10 m inutes immersion in 5 M N H 4OH plus Cu(N 03)2, and (b) high magnification o f an area shown in (a).
![Page 76: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/76.jpg)
61
¥£&&5w m & ^ $w a S S & s t f M g *
H R i8 ® ^ S t |8 f e s
KiSSSMffiSWEi
1 P ® §
F ig u re 19. Scanning electron m icrograph showing surface appearance o f a specimen after 10 minutes immersion in 0.1 M C u S 0 4 solution.
![Page 77: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/77.jpg)
T ab le 2. Strain-to-Initiation, Strain-to-Fracture and Slip Band Spacing o f a -B rassthe Different Environments.
Environment£ i S f
SBS(nm) at S f
Air — 0.932410.0065 1.310.3
0.1 M CuS04 0.030010.0002 0.803410.0054 1.210.5
1 M NaN02 0.0150+0.0005 0.380910.0065 1.510.4
5 M NH4+/Cu++ 0.005410.0001 0.099010.0032 1.510.4
All values are based on three measurements. £/ = strain for crack initiation £f = strain for fracture
![Page 78: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/78.jpg)
effects on the stress-strain behavior o f the material. Figures 20 (a)-(d) are electron
m icrographs o f typical fracture surfaces o f specimens tested in the three different SCC
solutions and in laboratory air. The values o f strain-to-crack initiation and strain-to-
failure consistently show that the NH4OH environment caused the m ost severe
embrittlement, w hereas the least susceptibility was shown in 0.1 M CuSOt. Table 2
also shows that the SBS at fracture was similar for all three environments as well as for
the experiments in laboratory air. Furtherm ore, Figure 21 provides m ore details on the
SBS developm ent at the initial stages o f straining and Figure 22 gives typical surface
appearances o f slip bands in these environments. It was evident in all o f these tests that
dense SBS o f about 1.5-2 pm had to develop prior to crack initiation. Also, the
presence o f the SCC electrolyte prom otes the development o f dense SBS in
com parison to straining in laboratory air.
Figure 23 presents the early stages o f the stress-strain behavior o f a -b rass in the
three electrolytes and in laboratory air. It is evident that the SCC environm ents cause a
strain hardening and its extent is consistent with the SCC susceptibility shown by the
material in these environments, Table 2. It was noted that for all three electrolytes a
certain degree o f strain hardening was required prior to SCC initiation corresponding
to a stress level o f about 3 .7 x l0 3 psi (25.5 M Pa).
Figure 24 presents the FWFIM measurem ents from XRD tests for specimens
that w ere strained by £t = 5% (total strain) in the three different electrolytes. FW HM
m easurem ents are also included for specimens strained in laboratory air. These results
show that for the same strain level, all three electrolytes produce a higher dislocation
density at the near-surface region compared to that developed in laboratory air.
Com paring the three SCC electrolytes, a much higher dislocation density develops in
NH4OH. In fact, the dislocation density developed by straining at £t = 5% in NH4OH is
![Page 79: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/79.jpg)
64
iftfCi'Jo .l m m
F igu re 20. Fracture surfaces produced by testing (a) in 5 M N H 4OH plus Cu(N 03)2, (b) in 1 M N a N 0 2) (c) in 0.1 M C u S 0 4 and (d) in laboratory air.
![Page 80: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/80.jpg)
SBS,
jx
m65
40
35
30
25
20
5
0
5
00 5 10 15 20 25
s T X 1 0 0 0
F ig u re 21. Slip band spacing developed during SCC testing in the three electrolytes (solid signs represent crack initiation).
![Page 81: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/81.jpg)
66
F ig u re 22. Typical surface appearance o f slip bands developed in the three electrolytes after testing for a total strain o f 0.006 in (a) 5 M N H 4OH with Cu(N 03)2, (b) 1 M N a N 0 2 and (c) 0.1 M C u S 0 4 solution.
![Page 82: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/82.jpg)
67
• y
2000
1000Air-
500000
1500
Figure 23. The early stages o f the stress-strain behavior o f a-brass in the three electrolytes and in laboratory air.
![Page 83: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/83.jpg)
RA/H
M68
Strain Broadening0.60
0.55 envronment
0.50
0.45
0.40
0.35
0.30
0.25
0.200 10 20 30 40 50
% strain
F ig u re 24. The full width half maximum (FW HM ) m easurem ents o f the {111} peak obtained by X-ray diffraction o f a -b rass specimens tested in different environments.
![Page 84: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/84.jpg)
69
equivalent (no statistical difference) to the one developed at fracture by straining in
laboratory air.
C. Dislocation Configuration During TGSCC
Figure 25 (a) illustrates typical dislocation configurations from the near-fracture
surface region o f TGSCC in an a -b rass single crystal. Intensified planar slip and
dislocation pile-ups on {111} planes w ere evident in areas close to the fracture surface.
In many cases the formation o f long stacking fault ribbons was also observed. In
contrast to the dislocation arrangement o f the near-fracture surface area, the dislocation
configuration observed in the pure mechanically deformed regions (masked gauge
section, w ith no environmental contact) was significantly different, Figure 25 (b).
D ispersed dislocations and a much lower dislocation density was observed in these
areas. Some dislocation pile-ups were present, but their number and density (number
o f dislocations/unit area) w ere substantially lower compared to those observed in the
SCC areas.
Several m icrocracks w ere also present on the fracture surface, Figure 26.
E lectron diffraction analysis showed that the microcracks were following a <211 >
direction, which is the orientation o f the intersection between the {111} and the {011}
crack plane. Thus, these m icrocracks m ore than likely are associated with the
form ation process o f crystallographic steps7,12 separating parallel and displayed {011}
TGSCC facets. It is characteristic to note that the walls o f the m icrocracks were very
sm ooth suggesting that they were formed by a highly localized process. During
TGSCC the thin ligaments connecting parallel and displayed cracks sustain most o f the
applied load and thus, have high shear stresses acting upon them. On the other hand,
owing to the presence o f the environment, the material undergoes embrittlement similar
to that observed during the TGSCC initiation process, producing {111} cracking.
![Page 85: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/85.jpg)
Figure 25. Dislocation configuration in an a-b rass SCC specimen (a) a region near the stress corrosion fracture surface showing intensified pile-ups on {111} slip planes and (b) a pure mechanically deformed region showing a more hom ogeneous dislocation distribution.
![Page 86: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/86.jpg)
71
5 t w
0.2 (Mm
Figure 26. A microcrack in a -b rass following the <211> direction (intersection o f the {111} with the {011} crack plane).
![Page 87: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/87.jpg)
In pure Cu, dislocation configurations in the TGSCC and pure mechanically
deform ed regions were, in general, o f a cellular structure, which is consistent with the
2 2 higher SFE o f this metal («90 mJ/m for pure Cu compared to «10 mJ\m for a-brass).
How ever, in the pure mechanically deformed areas, the dislocation density was lower,
the distribution was m ore diffused, Figure 27 (b), and indicated a rather hom ogeneous
deform ation mode. In areas close to the SCC surface, traces o f planar slip w ere found
within the dislocation cell walls, with the dislocations being m ore intensified, Figure 27
(a). Furtherm ore, m icrocracks with < 211> traces were also present on the stress
corrosion fracture surfaces. Similar to a-brass, relatively sm ooth m icrocrack walls
w ere also observed, Figure 28. Intense coplanar arrays o f dislocations w ere evident in
regions ju st ahead o f the tip o f such micro-cracks, Figure 28. The higher dislocation
density present on the m icrocrack walls in pure copper, Figure 28, com pared to that in
a-brass, Figure 26, is consistent with the significantly higher SFE o f copper. In
general, the facets o f the TG SCC steps in copper exhibit significant plastic deform ation
and a much less crystallographic character compared to those in a -b rass.95
![Page 88: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/88.jpg)
73
0.2 f i m
ytjauMaktfftusfoiffjyiiBiaMi
Figure 27. Dislocation configuration in a pure Cu SCC specimen (a) a region near the stress corrosion fracture surface showing cellular dislocations with traces o f planar slip in the walls o f the dislocation cells and (b) a pure mechanically deformed region showing a m ore hom ogeneous dislocation substructure.
![Page 89: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/89.jpg)
74
4, w - . y - « v y ^ n y ;y-: V ;> v T - f Y f y ' - a ' w , - y for: p, ;<■*P :%
Figure 28. Transmission electron m icrograph showing dislocation pile-ups associated with dissolution m icrocracks in pure copper. The m icrocrack tip is shown on the upper part o f the micrograph.
![Page 90: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/90.jpg)
CHAPTER VI. DISCUSSION
A. Deformation Evolution During TGSCC Initiation
1. Environment-Induced Surface Plasticity
In view o f the localized nature o f the deformation evolved during SCC in the
present w ork, the magnitude o f the plastic strain ( £s) was estim ated at the near-surface
region. Strain due to coarse slip can be calculated from the SBH (h) and the num ber o f
slip bands per unit length (N) by using the expression.147
w here N = 1/d w here d is the SBS. It should be noted that the strain calculated from
the above equation is independent o f the grain size o f the material. Table 3 provides
the calculated values o f near-surface strain as a function o f the bulk strain, SBH and
initiation ( £ / ) is equivalent to the strain-to-fracture required to produce ductile fracture
o f the material in air ( £ / = £ /= 0.75). This is further verified by the XRD
m easurem ents shown in Figure 24, where very similar dislocation densities were
obtained for specimens strained by only £t =5% in NH4OH (crack initiation had
occurred) and strained to fracture in laboratory air, £t = 49% . Thus, a fundamental
fracture criterion apparently exists (critical strain o r dislocation density for fracture) for
these ductile FCC materials, and environmentally-induced cracking is caused by
localizing the required strain for fracture. The reason that the near-surface strain starts
decreasing after some point, is that after crack initiation, m ost o f the strain is localized
(7)
slip band density. It is striking that the localized near-surface strain required for crack
75
![Page 91: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/91.jpg)
T ab le 3. Calculated Values o f N ear-Surface Region Strain.76
Bulk Straine
Slip Step Height h, pm
Slip Band Density N , |im"l
Near-SurfaceStrain
sc0.002 1.4 0.66 0.770.006 3.3 0.28 0.770.017 6.0 0.15 0.760.036 8.0 0.10 0.660.100 10.0 0.07 0.58
All values are based on three measurements.
![Page 92: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/92.jpg)
77
at the crack tip and the SBH may also be reduced due to dissolution at the slip steps.
Thus, after initiation the coarsening rate o f SBH is reduced (reaching a plateau around
14 pm, Figures 12 and 13) and neighboring slip bands coalescence producing larger
SBS at the near-surface region as shown in Figure 14.
Furtherm ore, the above values o f near-surface strain can be used to obtain a
rough estimate o f the number o f dislocations involved in the slip bands and the
dislocation density at the near-surface region by using the expression.148
ss = Nnbcp (8)
For ss = 0.77 (corresponding bulk strain &p = 0.002) the above equation produces n =
3 • 1 1 2 *6x10 dislocations and a dislocation density o f about 4x10 c m '. It is im portant to
note at this point that the above calculated dislocation density is in a complete
agreement with that determined independently by K ram er et al.95 (4 .5x10 11 cm’2) for
naval brass tested in CuS04 by using X-ray diffraction methods, in spite o f differences
in alloy com position and type o f electrolyte. In fact, several previous SCC studies149' 151
have shown that a high critical dislocation density develops in the near-surface region
prior to cracking. Similar effects have been observed in materials undergoing fatigue
cracking.13,14,152 Thus, in relation to the aforementioned fracture criterion, it can be
postulated that in general, fracture occurs when the total strain energy from the
combined stress field o f dislocations in the material reaches a critical limit relating to
the lattice decohesion. In SCC the critical dislocation density is localized and in the
ductile overload fracture distributed within the entire volume o f the material.
2. Effect of Anodic Dissolution
In an effort to assess the possible contribution o f the anodic dissolution to the
crack initiation process, an estimate o f the crack initiation rate (da/di) w as obtained.
The estimated rate was com pared with the experimentally observed rate o f about
![Page 93: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/93.jpg)
78
0.2 pm/s. Assuming that the first crack initiation event is due to anodic dissolution at
the slip bands, then
- = i — (9)dt zF p '
where i£ is the current density at the slip bands, M is the atomic weight o f the metal
(about 65 g/mole), 2 is the valence o f the solvated species ( 2 = 2), F is the Faraday's
constant (96500 C/mole) and p the density o f the material (7.13 g/cm 3 assuming Zn
dissolution). Even by assuming that the current density i6 is equivalent to the total
dissolution rate m easured during straining (6 .7 x l0 3 pA /cm 2), da/dt « 0 .3 x l0 '2 pm/s,
which is almost tw o orders o f magnitude lower than the experimentally observed crack
initiation rate for the present strain rate is obtained. The above analysis suggests that
indeed enhanced dissolution takes place at the emergent slip bands, but m ore than likely
dissolution alone cannot account for the crack initiation.
B. Effect of Electrolyte Type on TGSCC
The corrosion results from the three different electrolytes further foster the
above indication that crack initiation cannot be attributed to anodic dissolution alone.
The corrosion rate o f a -b rass in NaNCh was found to be by m ore than tw o and a half
orders o f m agnitude lower than the one in CuS04 (Table 1), however, the SCC
susceptibility in the form er solution was significantly higher (Table 2). Nevertheless,
the corrosion results clearly show that the application o f stresses can significantly
enhance anodic dissolution, especially in cases where passive films develop (Table 1).
The present results suggest that the role o f the environment is to cause strain
hardening. Figures 21, 23 and 24 show that SCC susceptibility is directly related to the
ability o f the environment to cause strain hardening and is consistent with the
![Page 94: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/94.jpg)
79
aforementioned fracture criterion o f critical strain energy. Strain hardening is
translated into dense SBS (Figure 21) and higher slope in the stress-strain response o f
the material (Figure 23) due to the developm ent o f higher dislocation density (Figure
24). Thus, in term s o f SCC susceptibility the three environments can be ranked as
N H 40H > NaNCte > CuS04.
The present results suggest that the ability o f the environment to cause SCC
initiation is related to its effectiveness in producing dense slip. For example, among the
three SCC electrolytes, C uS04 exhibits the slowest rate o f slip band density increase
(Figure 21) and therefore the lowest SCC susceptibility. In view o f the present results,
the role o f the environment in increasing slip band density can be attributed not to the
corrosion rate itself, but probably to the corrosion instabilities and patterning in the
dissolution process.
The dissolution o f alloys often occurs via the development and m otion o f a
rugged reaction front owing to the selective dissolution o f one or more elements. This
process is known as de-alloying and in the case o f a -b rass involves mainly Zn
dissolution. Early studies by W agner153 showed that, i f the rate-limiting step for such a
process is in the phase being consumed, geometrical instabilities develop along a planar
interface and grow exponentially with time. A similar situation was observed in
aggregation processes154 and this has been an area o f intense study.155' 157 A global
theoretical approach to the morphological instability phenomenon has been developed
by Santarini158 and application o f this model to dissolution 159 predicts the development
o f patterning in the mobile interface.
Some evidence o f dissolution patterning was observed in the present study
during the immersion tests in N H 4 OH, Figure 18, and that probably can account for the
fast development o f dense slip band spacing in this environment under stress.
Immersion in CuS04 was found to cause a rather random dissolution, Figure 19, that
![Page 95: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/95.jpg)
80
probably delayed the development o f dense slip spacing. Finally, exposure to NaNCte
w as found to cause passivation but under stress the film is ruptured selectively at
em ergent slip bands at the surface thus localizing dissolution and inducing a pattern that
consequently eases slip band development, Figure 22 (b).
C. Dislocation Arrangement During SCC
The present w ork provides further evidence that there is a difference in the
deform ation m ode betw een the areas directly in front o f the crack tip where an
environmental interaction exists and areas at larger distances (with no environmental
interaction). The deformation in both the non-ferrous FCC metals tested in the present
w ork w as found to be m ore localized (coplanar) in the TG stress corrosion crack tip
region and rather hom ogeneous in areas away from the grow ing crack, which is in
agreem ent with the previous TEM results in 304 austenitic stainless steel.117,160 In
principle, the above TEM observations are consistent with earlier studies95,151'161,152 and
with the results o f the present deform ation evolution study, where high dislocation
densities w ere observed in the near-surface region resulting from the environmental
action. It should be pointed out, that besides the higher dislocation density observed in
the vicinity o f the crack tip, the present results also indicate that the "stress-
environment interaction" modifies the dislocation configuration.
The results o f the present deform ation evolution study showed that slip is highly
localized, but on the other hand has a very coarse nature, too. The slip bands were
very sm ooth in appearance resembling that o f cleavage-like TG SCC surfaces. In
addition, from TEM observations during in situ crack tip deform ation o f FCC metals,
O hr163 reported that in the early stages o f straining, deform ation is coplanar, and a
transition to cellular arrays occurs only at larger strains. Thus, under normal
conditions, the area immediately ahead o f the stress corrosion crack tip, where the
strains are the largest, would be expected to display less dislocation planarity than areas
![Page 96: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/96.jpg)
81
further away from the crack tip where the strains are relatively low. However, the
opposite was observed in the present study, and thus, the present evidence is difficult to
reconcile with localized dissolution proposals.5
D. Crack Initiation and Propagation
The present w ork shows that besides the enhanced dislocation activity in the
near-surface region, the environment also modifies the deform ation pattern. The
environment-induced deform ation is characterized by finely-spaced, coarse slip bands,
in agreement with the TEM observations from areas just in front o f the crack tip in
three different FCC materials, namely 304 austenitic stainless steel117, a-brass, and pure
copper.164,165 In all o f the above studies it was observed that slip in front o f the crack
tip was localized (closely spaced slip bands) and m ore coplanar (coarse slip bands).
This evidence suggests that m ore than likely the latter deformation pattern develops
prior to each crack propagation event. Thus, since under the environmental action
planar dislocation arrangements are produced, the cracking process can be attributed to
the opening o f the pile-up when a critical deform ation localization (critical strain
energy) is reached. It has been shown in earlier treatm ents, that substantial local
stresses can be developed when a sufficient number o f dislocations join a pile-up.166
Thus, the normal stresses necessary to open the pile-up can be provided from the sum
o f the externally applied stress and the local stress generated from the dislocations in
the pile-up. Also, the possibility o f highly localized dissolution assisting the mechanical
opening should not be excluded.
D ue to its localized nature, this fracture process would be expected to produce
very flat (111} facets consistent with the present experimental evidence, Figure 17.
Also, the same mechanism can produce the crystallographic steps occurring on
alternating {111} segments and separating parallel but displaced {011} propagation
facets.7,8'12'167 There is no difference in the appearance between the presently obseived
![Page 97: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/97.jpg)
82
{111} crack initiation facets and the {111} step facets. The above reasoning seems to
provide also a plausible explanation for the observed patterning in the CIS, Figure 15.
The crack initiation patterning is developed since the combined stress field from a
num ber o f pile-ups on surrounding slip bands (one crack initiated for every three slip
bands in the present study) contribute to reach locally the critical stress required for
fracture.
The reason the crack initiation plane is different from the crack propagation
plane is probably that during the very first initiation event, slip occurs first on the
primary slip plane thus the environment-induced deform ation is pronounced on that
plane resulting in {111} crack initiation. As deform ation progresses, double (and
multiple) slip takes place and the environmental effect is occurring on all slip planes
modifying the local stress field and resulting in a new crack orientation on the {011}
plane. In the presence o f a crack obviously no {111} crack initiation is observed since
the crack tip stress intensity is high enough to produce double o r multiple slip as has
been experimentally verified.7,117 Slip in the latter case is not required to be as coarse
as in the first initiation event since a much higher stress intensity prevails. Similarly, no
{111} crack nucleation should be expected in cases where significant pre-straining
exists.
Thus, there seems to be no fundamental difference in the crack initiation and
crack propagation mechanisms but simply the differences in crack orientation and
appearance may be due to the pronounced slip on the primary slip plane during the very
first initiation event. This can explain the fact that {111} crack initiation facets are very
sm ooth and featureless (Figure 17), where crack propagation facets show evidence o f
em ergent slip traces.7,117,114,16/ However, {111} crack propagation may be possible in
materials where certain slip systems are blocked and gliding is allowed mainly on a
single slip system (i.e. martensite formation and preferential precipitation on certain
![Page 98: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/98.jpg)
83
{111} segments in austenitic stainless steels and A1 alloys, respectively), o r in materials
where the environment is prom oting enhanced gliding on the primary slip system that is
sufficient to cause fast crack grow th prior to the activation o f additional slip
system s.168,169 Regarding the crack advance distance, it is only logical to expect that
the crack will propagate in steps about equal to the depth o f the surface layer (o r the
region in front o f the crack tip) w ith high dislocation density (for TG SCC in P-brass it
has been determined to be 20-30 pm 151). The brittle character o f the fracture surface
can be accounted for by considering the coarse character o f deform ation within its
localization (Figure 14) that on a microscale is causing very little distortion in the
adjacent atomic structure o f the material (i.e. localized coarse slip on {111} planes).
In principle, the enhanced dislocation mobility observed during SCC in the
present and previous studies is similar to liquid metal embrittlem ent170 and hydrogen-
induced micro-plasticity.26,171 Coarse slip band formation during slow rate straining o f
Al-Li-Cu alloys that were pre-exposed in NaCl solution, a stage that presumably
produces hydrogen that enters the material has also been observed.172 These
observations tend to suggest that in all o f the above environm ent-assisted cracking
phenomena the role o f the environm ent is to reduce the activation energy for
dislocation nucleation and m otion, and also to coarsen the slip pattern as observed in
the present work.
E. Proposed Environment-Induced Deformation Localization Mechanism
Even though several TG SCC m odels10,110,114,173,174 have been proposed in the
past, no consensus has been reached yet regarding the nature o f the cracking process.
In view o f the present evidence, an environment-induced deformation localization
mechanism based on a vacancy-dislocation interaction process is being proposed.
The main elem ent o f the p resen t m echanism is that the environm ent induces
![Page 99: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/99.jpg)
84
nucleation o f dislocations from the surface region at loads well below those required
for normal yielding in air. This process is shown schematically in Figure 29. Vacancies
produced by anodic dissolution reduce the interatomic bond density at the surface
region, causing dislocation nucleation and out o f surface displacement. It has been
reported that extensive brass dealloying occurs on stressed surfaces175’176 and recently
m ore direct evidence o f anodic generation o f vacancies has been provided.177 The
present results further suggest that a periodicity in the dissolution process may be
critical in enhancing the development o f dense slip band spacing at the near-surface
region.
Very recently, the critical role o f the surface state in the dislocation nucleation
process was dem onstrated by Gerberich et al. 178 by conducting nanoindentation
studies. It w as shown that the load bearing capacity o f Fe-3wt% Si can be reduced by
tw o orders o f magnitude if the 10 nm thick native„oxide film is removed. Thus,
dislocation generation occurred at loads well below the normal plastic loading.
Similarly, the role o f the SCC environment can be thought o f as one o f creating a
surface state (corrosion patterning and periodicity) that prom otes dislocation emission
at loads below the elastic limit. In this case, vacancies reduce the interatom ic bond
density at the near-surface region facilitating nucleation o f dislocations, Figure 29. As
the process o f environment-induced dislocation emission continues, the local strain
from the accumulated dislocations reaches a critical level as described earlier and (111)
cracking occurs. It is important to point out that due to lower energy barrier for
dislocation nucleation during SCC, strain hardening (dislocation accum ulation and
interaction) is accelerated as was observed experimentally, Figures 23 and 24. After
initiation, the dislocation emission process is facilitated on more than one slip system
and the stress field is modified causing '{011} overall cracking, Figure 30.
![Page 100: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/100.jpg)
85
ooooooooooooooooooooooooooooooooooo
oooooooooooooooooooooooooooooooooo(b )
ooooooooooooooOOOOOtOoooooooooooooo
(<=)
ooooooooooooooOOOOt Ooooooooooooooo
(d)
oooooooooooooooo
oooooooo(«) ( 0
F ig u re 29. Schematic representation o f proposed environment-induced dislocation emission (a) perfect lattice; (b) vacancy generation due to anodic dissolution; (c) generation o f a dislocation and out o f surface displacement by one inter atomic distance;(d) and (e) formation o f planar dislocation arrangement; and (f) crack nucleation by opening o f a dislocation pile-up in a slip band.
![Page 101: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/101.jpg)
86
overa ll c rack ing p lane
d is locationnucleation
F ig u re 30. Schematic representation o f proposed multiple dislocation nucleation and fracture surface characteristics produced during crack propagation.
![Page 102: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/102.jpg)
87
Besides the induction o f dislocations from the material surface, the possibility
exists that vacancies can further interact with dislocations and also stress-assisted
vacancy diffusion may influence the propagation process. These tw o aspects are
further explored in the next sections.
1. Vacancy-Dislocation Interaction
Additional vacancy-dislocation interactions were explored in an effort to
provide a plausible explanation for the observed localization in the deform ation mode
during SCC. It takes into consideration earlier ideas expressed by Forty179 and
Jones.174 It is advocated that besides vacancy induction o f dislocations during the
crack initiation stage, vacancies produced by the anodic dissolution process at
emergent slip steps,5 migrate in the material and interact with dislocations in the near
crack tip region, modifying their configuration. The interaction o f vacancies with
dislocations has been previously discussed for both, the "good" lattice surrounding the
co re180 and the narrow core region consisting o f a highly distorted atomic structure.181
This subject is further reviewed by Ballufi et a l .1S2 Vacancies do not have much elastic
interaction with dislocations, but the electrical and other effects associated with the
absence o f an atom make up for this in most solids. Considering only the effect o f the
variations in charge density (z-z0)e that result from the volume dilatation, Cottrell et
al.m derived the following numerical expression for the electrical interaction energy
( Uelectr) between an edge dislocation (with a Burgers vector b) and a vacancy at
distance r :
U e le c tr * 0.02(z-zo)b/r, eV (10)
Positive vacancy binding energies ranging from 0.2 eV - 0.7 eV have been found for
both o f the above dislocation regions. Furthermore, positive vacancy binding energies
![Page 103: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/103.jpg)
have been determined in both the compressive and tension regions o f an edge
dislocation, indicating that vacancies can easily migrate tow ards the core region.
Thus, the initial vacancy injection at the surface region o f the crack tip is
visualized to be followed by vacancy attraction to the crack tip dislocations. Vacancies
are absorbed and eliminated on dislocation jogs causing dislocation climbing and
gliding around barriers that otherwise would impede dislocation m otion191 resulting in
faster dislocation accumulation thus reducing the time for strain hardening. The
interaction o f vacancies with dislocations prom oting glide is consistent with the
emergent slip bands consisting o f a cluster o f slip lines observed in the present w ork on
the specimen surfaces and the localized dissolution taking place at these sites that serve
as source for vacancies. Intense corrosion at emergent slip steps was observed for both
a -b rass and copper specimens in the present study.
It is important to note that the vacancy generation mechanism during corrosion
requires form ation o f kink and ledge sites at the crystal surface184 which are provided
by the slip process. As has been discussed earlier in the present study, corrosion
patterning and periodicity effects can produce finely spaced slip bands which
consequently can furnish the required ledges for vacancy formation. It has been
docum ented that intense slip bands are very prone to preferential dissolution due to the
influence o f the dislocation m icrostructure on the free enthalpy o f dissolution and the
energy o f activation.185 M ore importantly, vacancy formation and their adsorption by
dislocations is expected to take place very effectively since the corrosion process is
occurring on the slip bands. Thus, the environm ent/deform ation interaction involves
localization o f deformation by the environment and localization o f corrosion by slip.
There is further evidence for the above interaction from earlier w ork on Al, Cu
and Au single crystals by K ram er186 who observed lower activation energies for plastic
deform ation in tests under metal dissolution conditions. In fact, the decrease in the
![Page 104: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/104.jpg)
89
activation energy was consistent with the dissolution rate o f the metals and followed
the order Al > Cu > Au. Very recently, Jones and Jankow ski177 provided conclusive
evidence to an earlier proposal by Revie and Uhlig121 that anodic dissolution can
generate a supersaturation o f subsurface vacancies which form divacancies and migrate
in the material. These observations are consistent with the notion that corrosion-
induced vacancies prom ote plastic deformation. Thus, there is evidence suggesting
form ation o f corrosion-induced vacancies in FCC pure metals and alloys e.g. dealloying
o f brasses (dezincification o f SCC surfaces).177 In summary, the possible patterning in
metal dissolution seems to facilitate plastic deformation, which in turn favors formation
o f emergent slip bands that further enhance localized dissolution.
W hile the near-surface dislocation density increases, the vacancies that have
interacted with dislocations tend to prom ote a coplanar dislocation arrangement. This
can be envisioned to occur by a mechanism involving annihilation o f dislocation-
dislocation intersections and dislocation jogs by vacancies, since these sites can act as
sinks for absorbed vacancies. Furthermore, continuous supply o f vacancies to these
sites by dislocations (and diffusion) is expected due to the high subsurface vacancy
concentration produced by the corrosion process. Thus, the vacancy-induced
dislocation process, the migration o f divacancies and their interaction with dislocations
can account for the observed high dislocation density at the surface174’180 and the
localized deform ation mode observed in the present work. The sequence o f events
seems to be as follows: localization o f deformation under the environmental influence
(vacancy-induced dislocations due to corrosion patterning), localized dissolution at
emergent slip bands at the surface, vacancy generation which react to form divacancies 121
that migrate into the material, divacancy attraction by dislocations, easier dislocation
glide and build up o f high dislocation density, interaction o f divacancies with energetic
sites (dislocation intersections) and modification o f the dislocation configuration.
![Page 105: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/105.jpg)
90
2. Vacancy Contribution to Crack Propagation
It is pertinent at this point to refer to an early suggestion by Forty179 regarding a
TG SCC mechanism for a -b rass involving the interaction o f dislocations with a thin
elongated void on {111} produced by vacancies generated from dealloying. Forty also
considered a stress analysis by Fujita187 showing that if a thin void exists on the {111}
slip plane, then slip on this plane can force dislocations to join the slit and form a
hollow dislocation with a large Burgers vector (nh). Stress field analysis around this
hollow dislocation indicated that a substantial com ponent o f normal stress is acting
across the slip plane, that can lead to fracture when a sufficient num ber o f dislocations
(ri) jo in the hollow dislocation or when
nb = (Lh/2)1/2 (11)
L and h are the length and width o f the void, respectively. A similar expression was
developed earlier by S troh166 by considering a dislocation pile-up on a Lom er-Cottrell
L ock (LCL). U nder an effective shear stress (oa-oo) the maximum normal stress (om)
at a distance r from the lock is:
om = (ocr o0) (nb/r)1/2 (12)
Oa and oo being the applied shear stress and frictional stress, respectively. This concept
was adopted later by Kramer et al.95 who suggested that TGSCC occurs when the sum
o f the applied stress and the stress due to the accumulation o f dislocations reach the
fracture strength o f the material. M ore interestingly, the above stress field analysis191,192
showed that the direction o f maximum normal stress is not vertical to the slip plane but
it forms an angle o f about 70° with this plane. The implication o f this stress field
![Page 106: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/106.jpg)
91
geom etry is that after a certain length o f a nucleated crack, fracture may tend to extend
on a plane inclined to the {111} crack initiation plane, i.e. {011} plane.
In view o f the above discussion, we can further elaborate on the proposed
environment-induced deformation localization mechanism. Firstly, crack initiation
occurs by environmentally-induced strain localization on {111}, when a critical strain
energy is reached creating a fine slot on that plane. After crack initiation on {111}
plane, strain localization continues to occur in front o f the {111} slot and dislocations
start piling up. A gradually increasing normal stress develops in the surrounding region
as m ore dislocations join the pile up, with its maximum located along a direction
inclined at 70° from the {111}. At a certain point the stress intensity at the tip o f the
slot is high enough to activate the secondary slip plane and dislocations start piling up
on that {111} plane at 70.5° from the primary slip plane. The activation o f the
secondary slip system will modify the stress field, and under these conditions, the final
direction o f the stress (from both pile-ups) is approaching the direction normal to
{011} since this plane bisects the tw o slip planes. Thus, under the environment-
deform ation interaction localized slip and dissolution can occur simultaneously or in a
fast alternating sequence on both slip planes producing cleavage with an overall {011}
plane orientation, Figure 30, when a critical value o f strain energy is reached. Since the
m agnitude o f the critical tensile stress depends on the num ber o f dislocations in the pile
up, a direct relation between tendency to planar slip o r SFE and TGSCC susceptibility
is implied. Furthermore, tendency to planar slip will also correlate to the intensity o f
dissolution at slip steps and vacancy formation, since the latter mechanism requires
surface ledges184 that can be generated by the em ergent slip steps.
Cleavage on {011} is prom oted due to its particular crystallographic orientation
betw een the tw o {111} planes, low surface energy95 or to accum ulation o f vacancies
on this plane as suggested by Jones.177 It should be noted however, that the crack jump
![Page 107: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/107.jpg)
92
distances predicted by Jones could not comfortably be reconciled w ith the length o f
observed crack advance distances. However, in view o f the present results, it is evident
that a higher vacancy concentration may be produced in the plastic zone due to
enhanced vacancy transport along dislocations. Indeed, high rates o f vacancy diffusion
along dislocation cores can be reached due to the substantial reductions o f the vacancy
m igration energy in the highly disturbed core region.182 Thus, vacancies may also
contribute directly to the crack propagation process.
In an effort to explore further the possible contribution o f vacancies to the
embrittlement process, the divacancy diffusion in the high triaxiality region in front o f a
blunted crack tip is considered. Divacancies instead o f vacancies w ere considered due
to their higher stability and higher diffusivity.121 The basic argum ent used is, in
principle, similar to that proposed by N abarro for creep.188 In the presence o f an
applied tensile stress o, the free energy o f vacancy form ation is reduced by an amount
o fl (Q is the atom ic volume) producing a higher equilibrium vacancy concentration C :
C = C o e x p (o Q fk T ) (13)
C o being the thermal equilibrium concentration o f vacancies in the stress free region; T
the tem perature; and k the Boltzm ann’s constant. Thus, under stress, a net flow o f
vacancies can be realized due to the high concentration gradient betw een the vacancy
source (subsurface) and the highly stressed regime just in front o f the crack tip
(triaxiality region). The process followed here is very similar to the one used recently
to describe the stress-assisted grain boundary diffusion o f atomic hydrogen in Al-Li
alloys.189 First, Hill's model was adopted to describe the stress field ahead o f a blunted
crack tip, Figure 31(a) (see Appendix B for appropriate equations and values used).
![Page 108: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/108.jpg)
93
Then, Van Leeuwen's equation was modified to describe the diffusion o f divacancies in
the presence o f a stress field as follows:
dt v cPxd a dCv
R T dx dx (14)
v denoting divacancies and Vv the equivalent partial molar volume o f divacancies. By
assuming typical values for a-brass, such as a waiting time for crack advancement o f
60 s (experimentally observed SCC velocity «10 '7 m/s and crack jum p distance o f 6 p
m), the transient concentration profile o f divacancies was determined by solving
equation 4 numerically with Finite Difference. Figure 31(b) shows the transient
concentration profiles for stress-free (600 s) and stress-assisted (60 s and 600 s)
diffusion. For the stress-free case only the transient profile for 600 s is shown, since
the profile for 60 s was very shallow (penetration distance «2000 A) and for practical
purposes is not shown on the graph. The analysis shows that the presence o f the stress
field prom otes significantly the divacancy diffusion in the plastic zone. For a typical
waiting time o f 60 s, the divacancy diffusion zone extends almost 2 pm in front o f the
crack tip. Furtherm ore, based on the present analysis an additional beneficial effect on
divacancy m igration should be anticipated from the local stress field generated by the
dislocation pile-ups on the crack initiation slot.
It is interesting to note that recent creep experiments with planar copper-
sapphire interfaces tested in tension,190 showed the existence o f crystallographic
cavities at the interface, with cavity surfaces close to {110}. These observations
indicate that under stress, vacancies may have a tendency to accum ulate on specific
planes. The reason for that preference is not known at the moment, but it may relate to
the low atomic density o f {011}, its low surface energy and/or the particular geometry
![Page 109: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/109.jpg)
94
a800 i
0 0 4 0 0 -
200 -Elast i cZo n e
P las t i cZ on e
2 5155 10 200x, pm
bElast i cZ on e— Plas t i c
Zone
T r a n s i en t Prof i le6 0 s 6 0 0 s
S t r e s s F r e eCJ
x
S t r e s s As s i s t e d0 . 5
0.01050
x, pjm
F ig u re 31. (a) Stress distribution in front o f a blunted crack in a-brass; (b) Transient divacancy concentration profiles o f stressfree (600 s) and stress-assisted (60 s and 600 s) diffusion (Cs denotes the divacancy concentration at the su rface ).
![Page 110: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/110.jpg)
95
o f deformation. The {110} plane bisects the tw o {111} slip planes and vacancy
accumulation on {O il} , while these tw o planes are active, may cause maximum strain
relaxation. I f this is indeed the case, and under stress divacancies tend to accum ulate on
{110} planes in the diffusion zone, then embrittlement can be easily induced due to
highly localized alternating slip on this plane and due to the significant reduction o f
local fracture toughness in the embrittled zone. Also, the crack velocity in such an
"embrittled zone" is expected to be high enough for the crack to propagate for a
distance longer than the divacancy diffusion zone (m ore than likely up to the size o f the
plastic zone, 6 pm). Due to the stress triaxiality in this region, significant amount o f
plastic deform ation should not occur once a crack has initiated. Crack arrest can occur
at a preexisting slip band and the process is repeated. It should be noted that after the
first crack initiation event, less anodic dissolution will be required at slip bands because
as the crack gradually advances the stress intensity is increasing in front o f the crack tip
thus, a smaller number o f dislocations will be required in the pile-ups to reach the
critical stress for cracking. Finally, it should be pointed out that the environment-
induced deformation localization TGSCC mechanism described in the present work, is
compatible with the phenomenology o f cracking in non-ferrous FCC metals.
![Page 111: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/111.jpg)
CHAPTER VII. CONCLUSIONS
The results o f the present study showed that an environment-induced
deform ation localization pattern evolves at the near-surface region o f the material prior
to TGSCC. The near-surface strain required for SCC w as found to be equivalent to
strain needed for ductile fracture o f the material in air indicating the existence o f a
fundamental fracture criterion. Also, a patterning in the crack initiation process was
observed. In view o f the present results, TG SCC can be interpreted as localized
fracture under the sum o f the externally applied stress and the stress resulting from the
neighboring dislocation pile-ups lying on different slip planes that are accumulated in
the surrounding slip bands. The role o f the environment can be thought o f as that o f
causing a local reduction in the energy barrier for dislocation nucleation, thus causing
faster strain hardening com pared to behavior in laboratory air. This environment-
induced dislocation process can be attributed to the presence o f vacancies that reduce
the density o f the interatom ic bonds at the near-surface region, facilitating dislocation
emission.
Based on the present experimental observations and the phenom enology o f
TG SCC in non-ferrous FCC metals, an environment-induced deformation localization
mechanism is presented. M ore specifically, the suggested mechanism involves the
following events:
a) D ue to corrosion instabilities and patterning, deform ation localization occurs
via a vacancy-induced dislocation process and dense but coarse emergent
slip bands are produced at the specimen surface;
b) localized anodic dissolution occurs at emergent slip bands thus generating
subsurface vacancies;
96
![Page 112: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/112.jpg)
c) vacancies are attracted by dislocations, ease dislocation mobility and cause
a high dislocation density at the near-surface region further localizing slip;
d) a crack is nucleated on {111} slip planes when a critical strain energy is
reached from the externally applied stress and the stress from the
surrounding dislocation pile-ups;
e) in the presence o f a crack, the same process is repeated, but since relatively
high stress intensities prevail, multiple slip occurs that modifies the stress
field causing cracking on {O il} ; Stress-assisted diffusion o f vacancies may
assist the cleavage process by reducing the local fracture toughness;
f) the crack propagates in steps about equal to the depth o f the zone with high
dislocation density and finally is arrested at a pre-existing slip band. The
process is repeated and, as the crack advances, less dissolution is required
since the stress intensity is gradually increased and a smaller num ber o f
dislocations is required to reach the critical stress for cracking.
![Page 113: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/113.jpg)
CHAPTER VIII. SUGGESTED FUTURE RESEARCH
Future research is recom mended on the initial stages o f corrosion (instability
and patterning) in the absence and presence o f stress. The in situ X -Ray diffraction or
extended X-Ray absorption fine structure (EXA FS) spectroscopy may be employed to
study the surface disorder (instability) caused by electrolytes alone and by combination
o f electrolytes and stress. TEM examinations on stress free foils after different period
o f immersion tests can reveal the dislocation density and configuration changes resulted
from pure electrochemical reactions. This will clarify the role o f the SCC environment
in enhancing the dislocation density at the near-surface region.
98
![Page 114: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/114.jpg)
REFERENCES
1. Parkins Symposium on Fundamental Aspects o f Stress Corrosion Cracking, (TM S-AIM E, W arrendale, PA, 1992).
2. Corrosion-Deform ation Interactions, (les editions de physique, Paris, France, 1993).
3. F. A. Champion, Symp. on Internal Stresses in Metals and Alloys, (Inst, o f M etals, London, 1948),p .468.
4. H. L. Logan, J. Res. Natl. Bur. Stand. 48, 99 (1952).
5. R. W. Stahele, The Theory o f Stress Corrosion Cracking in Alloys, (NATO, Brussels, 1971), p .223.
6. E. I. M eletis and R. F. H ochm an , Corrosion 40, 39 (1984).
7. E. I. M eletis and R. F. Hochman, Corros. Sci. 24, 843 (1984).
8. E.I. M eletis and R.F. Hochman, Corros. Sci. 26, 63 (1986).
9. J.A. Beavers and E.N. Pugh, Metall. Trans. 11 A, 809 (1980).
10. K. Sieradzki and R. C. Newman, Phil. Mag. A51, 95 (1985).
11. B. D. Lichter, W. F. Flanagan, J. B. Lee and M. Zhu, Environment-Induced Cracking o f Metals, (NACE, Houston, TX, 1990),p .251.
12. E.N . Pugh, Corrosion 41, 517 (1985).
13. I. R. Kramer, C. R. Feng, and B. Wu, Mater. Sci. Eng. 80, 37 (1986).
14. I. R. Kramer, and S. W eissmann, Proceedings o f the Symposium on Novel Non-Destructive Evaluation Methods for Materials, (TM S-AIM E, W arrendale, PA, 1982), p. 141.
15. “Bibliography on Season Cracking” , Proc. Amer. Soc. Test. Mater. 41, 918 (1941).
16. G.A. Nelson, Bull. Amer. Soc. Test. Mater. 240, 39 (1959).
99
![Page 115: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/115.jpg)
10017. H. M oore, S. Beckinsale, and C. E. Mallinson, J. Inst. Met. 25, 35 (1921).
18. C. E. Stromeyer, J. Iron Steel Inst. 79, 404 (1909).
19. J. H. Andrew, Trans. Faraday Soc. 9, 316 (1913).
20. E.B. Wolff, J. Iron Steel Inst. 96, 137 (1917).
21. A. A. Griffith, Phil. Trans. Roy. Soc. A221, 163 (1920).
22. E. H. Dix, Trans. Inst. Metals Div. AIM E 137, 11 (1940).
23. F. H. Keating, Internal Stresses in Metals and Alloys, (Institute o f M etals. London, 1948), p .311.
24. U. R. Evans, Corrosion 7, 238 (1951).
25. A. R. Troiano, Trans. Amer. Soc. Metall. 52, 54 (1960).
26. C. D. Beachem , Metall. Trans. 3, 437 (1972).
27. I. M . Bernstein and A. W. Thompson, eds., Hydrogen in Metals, (Amer. Soc. for M etals, M etals Park, Ohio, 1974).
28. T. M atsum oto, J. Eastm an and H. K. Bimbaum, ScriptaMetall. 15, 1033 (1981).
29. T. Tabata and H. K. Bim baum , Scripta Metall. 17, 847 (1983).
30. T. Tabata and H. K. Birnbaum, Scripta Metall. 18, 231 (1984).
31. T. Tabata and H. K. Bim baum , Japan Inst, o f Metals 2 4 ,485 (1985).
32. I. M. R obertson and H. K. Bimbaum, ActaMetall. 3 , 353 (1986).
33. D. Shih and H. K. Bimbaum, Modeling Environmental Effects on Crack Growth Processes, (ASTM , Philadelphia, PA, 1986).
34. H. K. Birnbaum, I. M. Robertson, G. Bond and D. Shih, Proceedings o f the 11th International Congress on Electron Microscopy, (Japan Society o f E lectron M icroscopy, Tokyo, Japan, 1986), p .971.
35. G. Bond, I. M. Robertson and H. K. Birnbaum, ActaMetall. 3 5 ,2289 (1987).
![Page 116: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/116.jpg)
10136. G. Bond, I. M. Robertson and H. K. Bim baum , ActaMetall. 36, 2193 (1988).
37. A. S. Tetelman, Fracture o f Solids, C.D. D rucker and J.J. Gilman, eds., (Interscience, N ew Y ork 1963), p .671.
38. K. Farrell, J. Iron Steel Inst. 203, 71 (1965).
39. R. Gibala, Trans. Metall. Soc. A IM E 293, 1574 (1967).
40. C. M. Sturges and A. P. M iodownik, ActaMetall. 17, 1197 (1969).
41. E. Conophagos, J. Plusquellec, P. Azou and P. Bastien, L ’Jydrogene dans lesMetaux, (Congres International, Editions Science et Industrie, Paris, 1972), p .97.
42. N. A. Tiner, T. L.M ackay, S. K. Asimmaa and R. G. Ingersoll, Trans. Amer. Soc. Metals 61, 195 (1968).
43. S. P. Rideout, M. R. Louthan, Jr. and C. L. Selby, A STM STP. No.397, 137 (1966).
44. G. W. Powell, J. D . Braun, K. S. Chaney and G. L. Downs, Corrosion 26, 223 (1970).
45. M. R. Louthan, Jr., D. E. Rawl, Jr. and R. T. Juntoon, Corrosion 28, 172 (1972).
46. H. G. Vaughn and M. E. D eM orton, Brit. Welding J. 4 ,40 (1957).
47. P. Cotterill, Progr. Mat. Sci. 9, 41 (1961).
48. K. V. Popov and E. P. Nechai, Fiz. Khim. Mek. Mater. 3, 631 (1967).
49. C. V. Ow en and T. E. Scott, Metall. Trans. 3, 1715 (1972).
50. D .G . W estlake, Trans. ASM 62, 1000 (1969).
51. S. Gahr, M. L. G rossbeck and H. K. Birnbaum, Acta Metall.25, 135 (1977).
52. M. L. Grossbeck and H. K. Bimbaum, ActaMetall. 25, 125 (1977).
53. N. Narita, C. A ltstetter and H.K. Birnbaum, Metall. Trans. A 13A, 135 (1982).
![Page 117: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/117.jpg)
10254. T. B. Flannagan, N. B. M ason and H. K. Bimbaum, Scripta Metall. 15, 1355
(1981).
55. H. K. Bimbaum, J. Less Common Metals 103, 31 (1984).
56. B. Baranowski, Hydrogen in Metals II, (Paris, France, 1977), p.409.
57. M .L. Grossbeck and H.K. Birnbaum, ActaMetall. 25, 125 (1977).
58. S. Takano and T. Suzuki, Scripta Metall. 22, 265 (1974).
59. J. C. M. Li, R.A. Oriani and L.S. Darken, Zeits. Physik. Chemie. Neue Folge49, 271 (1966).
60. W. H. Johnson, Proc. Roy. Soc. Lond. 23, 168 (1874).
61. N . S. Stoloff, Environment-Sensitive Fracture o f Engineering Materials, (TM S- AIM E, W arrendale, PA, 1979), p.486.
62. W. R ostoker, J. M. M cCaughey and M. M arkus, Embrittlement by Liquid Metals, (V an Nostrand-Reinhold, N ew York, 1960).
63. M .H. Kamdar, Prog. Mater. Sci. 45, 1 (1973).
64. N. J. Kelly and N. S. Stoloff, Metall. Trans. 6A, 159 (1975).
65. A. R. C. W estw ood and M. H. Kamdar, Philos. Mag. 8, 787 (1963).
66. N .S. S to loff and T.L. Johnson, ActaMetall. 11, 251 (1963).
67 J. C. G rosskreutz and D. K. Benson, Surface and Interfaces, (Syracuse University Press, Syracuse, N .Y ., 1967).
68. R. M. Latanision, R.I.A .S. Tech. Rep., 72-22C, M artin M arietta Corp., Baltimore, M D (1972).
69. Y. Cheng, and C. Laird, Mater. Sci. Eng. 51, 111 (1981).
70. H. M ughrabi, Mater. Sci. Eng. 33, 207 (1978).
71. H. Spaehn, Environment-Induced Cracking o f Metals, (NACE, H ouston, TX, 1990), p.449.
![Page 118: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/118.jpg)
10372. H. J. Gough, J. Inst. Metals 49, 17 (1932).
73. J. Congleton, R. A. Olieh and R. N. Parkins, Metals Tech. 9, 94 (1984).
74. D. W hitwham and U. R. Evans, J.I.S.I. 165, 76 (1950).
75. K. Laute, Oberflachentech 10, 281 (1933).
76. H. N. H ahn and D. J. D uquette, Metall. Trans. 10A, 1453 (1979).
77. E. I. M eletis, J. Mater. Eng. 11, 159 (1989).
78. E. I. M eletis, and K. Lian, Wear-Corrosion Interactions in Liquid Media, A. A. Sagues and E. I. M eletis, eds., (TM S-A IM E, W arrendale, PA, 1991), p. 139.
79. E. I. M eletis, C. A. Gibbs and K. Lian, Dent. Mater. 5 ,4 1 1 (1989).
80. K. Lian, Effect o f Sliding Wear on Corrosion Behavior o f Dental Amalgams, M .S. Thesis, 1991.
81. E. I. M eletis, Scripta Metall. Mater. 24, 2375 (1990).
82. T. R. Pinchback, S. R. Clough and L. A. Heldt, Corrosion 12, 467 (1976).
83. S. Torchio, Corros. Sci. 26, 1933 (1986).
84. A. Kaeashima, A. K. Agrawal and R. W. Staehle, J. Electrochem. Soc., 124,1822(1977).
85. H. W. Pickering and P. J. Byrne, Corrosion 2 9 , 325 (1973).
86. M .G. Alvarez, M. G iordano, C. M anfredi and J.R. Galvele, Corrosion 4 6 , 717(1990).
87. R. N. Parkins and N. J. H. Holroyd, Corrosion 3 8 , 245 (1982).
88. S. Torchio, Corros. Sci. 21, 59 (1981).
89. V. K. Gouda, H. A. El-sayed, S. M. Sayed and G. M. Sherbini, Corrosion 3 8 ,
609(1982).
90. A STM B 154-73 Annual B ook o f ASTM Standards, Part 6, ASTM ,Philadelphia, PA, p .325 (1974).
![Page 119: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/119.jpg)
104
91. S.A. Bradford and T. Lee, Corrosion 34, 96 (1978).
92. Y. Xu, G. Thom pson and G C. W ood, Corros. Sci. 27, 141 (1987).
93. J. Yu and R.N . Parkins, Corros. Sci. 27, 159 (1987).
94. H. C. Shih and R. J. Tzou, Environment-Induced Cracking o f Metals, (NACE,Houston, TX, 1990), p.389.
95. I. R. Kramer, B. W u and C. R. Feng, Mater. Sci. Eng. 82, 141 (1982).
96. U.R. Evans, Symposium on Internal Stresses in Metals and Alloys, (Inst.M etals, London, 1947), p .291.
97. E. H. Dix, Proc. Amer. Soc. Test. Mater. 41, 928 (1941).
98. E. M attesson, Electrochim. Acta 3, 279 (1961).
99. E. N. Pugh and A. R. C. W estw ood, Phil. Mag. 13, 167 (1966).
100. E. N. Pugh, Environment-Sensitive Mechanical Behavior, A.R.C. W estwook, and N.S. S toloff eds., (G ordon & Breach, N ew York, 1966), p .351.
101. U. Bertocci and E. N. Pugh, Proceedings o f the 9th International Conference on Metallic Corrosion, (National Research Council, O ttawa, Toronto, 1984), p. 144.
102. E. M attsson and J. O. Bockris, Trans. Faraday Soc. 55, 1568 (1959).
103. U. Bertocci, and D. D. W agman, Standard Potentials in Aqueous Solution, A. Bard, R. Parsons and J. Jordan eds., (M. Dekker, N ew York, 1985), p.287.
104. G. W. Tindall and S. Bruckenstein, Anal. Chem. 40, 1402 (1968).
105. H. Gerischer and Z. Physik, Chem. 202, 302 (1953).
106. H. M atsuda and Y. Ayabe, Z. Elektrochem. 63, 1164 (1959).
107. H.L. Logan, J. Res. Mail. Bur. Stds. 48, 99 (1952).
108. A. J. M cEvily and A. P. Bond, J. Electrochem. Soc. 112, 131 (1965).
![Page 120: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/120.jpg)
105109. P. R. Swann and H. W. Pickering, Corrosion 19, 369 (1963).
110. J. R. Galvele, Corros. Sci. 27, 1 (1987).
111. J. R. Galvele, Corrosion-Deformation Interactions, (les editions de physique, Paris, France, 1993), p. 83.
112. W. F. Flanagan, P. Bastias and B. D. Lichter, ActaMetall. 38, 1313 (1990).
113. W. Flanagan, L. Zhong and B. D. Lichter, Metall. Trans. 24A , 553 (1993).
114. T. Magnin, R. Chieragatti and R. Oltra, ActaMetall. 38, 1313 (1990).
115. T. M agnin and J. Lepinoux, Fundamental Aspects o f SC C , (TM S, W arrendale, PA, 1991), p .323.
116. T. M agnin, Tenth International Conference on the Strength o f Materials,(The. Japan Institute o f M etals, Japan, 1994), p .25.
117. S. Jani, M. M arek, R. F. Hochm an and E. I. M eletis, Metall. Trans. 22A, 1453 (1991).
118. J.M . Silcox and P.R. Swann, Mechanics o f Environment Sensitive Cracking o f Materials, (The M etals Society, London, 1977).
119. J. A. Honkasalo and H. E. Hanninen, ibid., p.83.
120. A. J. A. M om, R. T. Dencher, C. J. W ekken and W. A. Schultze, ASTM STP665, p.305, (1979).
121. R. W. Revie and H. H. Uhlig, Acta Metall. 22, 619 (1974).
122. R. W. Revie and H. H. Uhlig, Corrosion Sci. 22, 669 (1972).
123. H. H. Uhlig, J. Electrochem. Soc. 123, 1699 (1976).
124. M. Smialowski and J. Kostanski, Corros. Sci. 19, 1019 (1979).
125. M. C. Petit and D. Desjardins, Stress Corrosion Cracking and Hydrogen Embrittlement o f Iron-Base Alloys, R. W. Staehle, ed., (NACE, H ouston, TX, 1977), p. 1204.
126. H. N. Hahn and D. J. Duquette, Acta. Metall. 26, 279 (1978).
![Page 121: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/121.jpg)
106127. D. A. Jones, C. D. Kim and B. E. W ilde, Corrosion 33, 50 (1977).
128. R. N. Parkins, ASTMSTP 665, 5 (1979).
129. R. N. Parkins and B. S. Greenwell, Metal Science, A ugust/Septem ber, 405 (1979).
130. I. R. Kramer, Corrosion 30, 383 (1975).
131. I.R. K ram er and A. Kumar, Proc. 2nd Int. Conf. on Corrosion Fatigur,(NACE, H ouston, TX, 1972), p. 146.
132. E. N. Pugh and A. S. Sedricks, Surfaces and Interfaces, V o I . n , (Syracuse University Press, Syracuse, NY , 1968), p. 183.
133. K Kamachi, T. O tsu and S. Obayaski, Trans. Jpn. Inst. Metall. 35, 64 (1971).
134. R. M. Yanici, Ph.D. Dissertation, R utgers University, 1982.
135. M. T. H ahn and E. N. Pugh, Corrosion 36, 380 (1980).
136. B. D. Lichter, T. B. Cassagne, W. F. Flanagan and E. N . Pugh, Microstr. Sci.13, 361 (1985).
137. F.C. Althof, Zeitshrift furMetallkunde 36, 177, (1944).
138. F. A. C otton and G. W ilkinson, Advanced Inorganic Chemistry, (Interscience, N ew York, 1962), p.756.
139. E. N . Pugh and A. R. C. W estw ood, Stress Corrosion Testing, A STM STP 425, p .228, (1967).
140. R. L. Fleischer, Acta. Metall. 8, 598 (1960).
141. G..A. Somoijai and M .A. Van Hove, Structure and Bonding, J. D. Dunitz et at., eds.,(Springer, Berlin, 1979).
142. J. Sokolov, F. Jona, and P.M . M arcs, Phys. Rev. B 31, 1929 (1985).
143. J. D. Eshelby, F. C. Frank and F. R. N. Nabarro, Phil. Mag. 42, 351 (1951).
144. J. Yu, R. N. Parkins, Y. Xu, G. Thom pson and G.C. W ood, Corros. Sci. 27,141 (1987).
![Page 122: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/122.jpg)
145.
146.
147.
148.
149.
150.
151.
152.
153.
154.
155.
156.
157.
158.
159.
160.
161.
162.
163.
107R. Arm strong, I. C odd and R. M. Douutwaite, Phil. Mag. 45, 7 (1962).
A. Parthasarathi and N. W. Polan, Metall. Trans. 13A, 2027 ((1982).
D. M cLean, J. Inst. Metall. 80, 507 (1951).
D. Li and X. M ao, Metall. Trans. 23A, 2873 (1992).
C. F. Lo, W. E. M ayo and S. W eissmann, CORROSION/88, paper no. 282, (N A CE International, H ouston, TX, 1988).
K. Kamachi, T. O tsu and S. Abayashi, Trans. Jpn. Inst. Metall. 35, 64 (1971).
D. B. Kasul, C. L. W hite and L. A. Heldt, Proceedings o f the Conference on Environment Induced Cracking o f Metals, (NACE International, H ouston, TX, 1990), p.219.
R. N . Pangbom , S. W eissmann and I. R. Kramer, Metall. Trans. 12A, 109 (1981).
C. W agner, J. Electrochem. Soc. 101, 225 (1954).
W. W. M ullins and R. F. Sekerka, J. Appl. Phys. 35, 323 (1963).
T. A. W itten and L. M. Sander, Phys. Rev. Lett. 47, 1400 (1981).
P. M eakin, Phys. Rev. A 27, 604 (1983).
R. M. Brady and R. C. Ball, Nature, Lond. 309, 225 (1984).
P. G. Santarini, J. de chimie phys. 82, 49 (1985).
P. G. Santarini, J. de chimie phys. 82, 329 (1985).
S. Jani, M. M arek, R.F. Hochm an and E.I. Meletis, Environment-Induced Cracking o f Metals, (NACE, Houston, TX, 1990), p.219.
K. Kamachi, T. O tsu and S. Obayashi, Trans. Jpn. Inst. Metall. 35, 64 (1971).
M. J. Kaufman and J. L. Fink, ActaMetall. 36, 2213 (1988).
S. M. Ohr, Mater. Sci. Eng. 72, 1 (1985).
![Page 123: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/123.jpg)
164.
165.
166.
167.
168.
169.
170.
171.
172.
173.
174.
175.
176.
177.
178.
179.
108E. I. M eletis, K. Lian and W. Huang, Proceedings o f the International Confeerence on CORROSION-DEFORMATIONINTERACTIONS, (Les Editions de Physique, Les Ulis, France, 1993), p .69.
E. I.M eletis and K. Lian, J. Mech. Behav. Mater. 6, 69 (1995).
A. N. Stroh, Proc. R. Soc. 223, 404 (1954).
W. F. Flanagan, M . W ang, M. Zhu and B. D. Lichter, Metall. Trans. 25A,1391 (1994).
Li Shiqiong, J. I. D ickson, J. P. Bailon and D. Tromans, Mater. Sci. Eng. 119, 59 (1989).
J. I. Dickson, Li Shiqiong, J. P. Bailon, and D. Tromans, Proceedings o f the Symposium on: Fundamental Aspects o f Stress Corrosion Cracking, (TM S- AIM E, W arrendale, PA, 1992), p. 3 03.
S. P. Lynch, Acta Metall. Mater. 29, 325 (1981).
H. K. Bim baum , Proceedings o f the Conference on Environment-Sensitive Fracture o f Engineering Materials, (TM S-AIM E, W arrendale, PA, 1979), p .326.
E. I. M eletis, and W. Huang, Mater. Sci. Eng. 148 A , 197 (1991).
W. F. Flanagan, P. Bastias and B. D. Lichter, ActaMetall. Mater. 39, 695(1991).
D. A. Jones, Metall. Trans. 16A, 1133 (1985).
T. R. Pinchback, S.P. C lough and L.C. Heldt, Metall. Trans. 6A, 1479 (1975).
T. R. Pinchback, S.P. Clough and L.C. Heldt, Metall. Trans. 7A, 1241 (1976).
D. A. Jones and Jankowski, Scripta Metall. Mater. 29, 701 (1993).
W. W. Gerberich, S. K. Venkataram an, H. Huang, S. E. H arvey and D. L. Kohlstedt, ActaMetall. Mater. 43, 1569 (1995).
A. J. Forty, Physical Metallurgy o f Stress Corrosion Fracture, (Interscience, N ew York, 1959), p .99.
![Page 124: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/124.jpg)
109180. R. Boullough and R. C. New m an, Rep. Prog. Phys. 33, 101 (1970).
181. M. Doyam a and R.M .J. Cotterill, Suppl. Trans. Japan Inst. Met. 9, 55 (1968).
182. R.W . Ballufi and A.V. Granato, Dislocations in Solids, F.R.N. Nabarro, ed., Vol. 4, Chapter 13, (North-Holland, 1979).
183. A. H. Cottrell, S. C. H unter and F. R. N . N abarro, Phil. Mag. 44, 1064 (1953).
184. H. W. Pickering and C. W agner, J. Electrochem.Soc. 114, 698 (1967).
185. B. Yan, G. Farrington and C. Laird, ActaMetall. 33, 1533 (1985).
186. I. R. Kramer, Trans. Metall. Soc. AIME 230, 991 (1964).
187. F. E. Fujita, ActaMetall. 6, 543 (1958).
188. H. G. VanBueren, Imperfections in Crystals, (North-Holland, Amsterdam, 1960), p .236.
189. T.I. Zohdi and E.I. M eletis, Scripta Metall. Mater. 26, 1615 (1992).
190. C. M. Kennefick and R. Raj, ActaMetall. Mater. 40, 615 (1992).
![Page 125: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/125.jpg)
APPENDIX A. NOMENCLATURE
110
![Page 126: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/126.jpg)
£f strain to fracture in air
et
et
ep
es
escc
<uvw>
{hkl}
ANOVA
BCC
CAC
CF
CIS
da/dt
J-'corr
EXAFS
F
FCC
near-surface strain for crack initiation
total strain
strain for crack initiation
plastic strain
near-surface plastic strain
strain-to-failure under stress corrosion cracking
indices for a family o f crystallographic directions
M iller indices for a family o f crystallographic planes
analysis o f variance
body-centered cubic crystal structure
corrosion-assisted cleavage
corrosion fatigue
crack initiation spacing
crack initiation rate
open circuit corrosion potential
extended X-ray absorption fine structure
Faraday’s constant (96500 C/mole)
face-centered cubic crystal structure
![Page 127: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/127.jpg)
FW HM : full-width at half maximum
GLM : general linear models procedure
H C P : hexagonal close-packed crystal structure
H E : hydrogen embrittlement
IG : intergranular
Ki : stress intensity factor
Kic : plane strain fracture toughness for m ode I loading
Kiscc : threshold stress intensity factor for stress corrosion cracking
LEED : low-energy-electron-diffraction
LM E : liquid metal embrittlement
SBH : slip band heights
SBL : slip band length
SBS : slip band spacing
SCC : stress corrosion cracking
SCE : saturated calomel electrode
SEM : scanning electron microscopy
SFE : stacking fault energy
TEM : transmission electron m icroscopy
TG : transgranular
W CC : w ear-corrosion cracking
XRD : X-ray diffraction
![Page 128: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/128.jpg)
APPENDIX B. HYDROSTATIC STRESS AND PLASTIC ZONE CALCULATION
113
![Page 129: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/129.jpg)
The hydrostatic stress in the plastic zone ( Op) immediately ahead o f a blunted crack o f a radius p is given by:
Op = O y[ln (l+ x /p) + 1/2]
w here O y is the material's yield strength and x is the distance in front o f the crack tip. The size o f the plastic zone (rp) is given by:
rp = (l/6 n )(k ISCC/ Oy)2
The values o f the various param eters used to determine the stress distribution and the divacancy concentration profiles (Fig. 31) are as follows: oy = 216 M Pa, p - 0.6 pm,
f p = 6 pm , V = 0.3, D v = lx lO ’16 m2/s, k ]SCC = 2.3 M Pam 1/2, Vy = 9 .16X10-6 m3/mol.
![Page 130: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/130.jpg)
APPENDIX C. POTENTIODYNAMIC TEST RESULTS OF a-BRASS IN DIFFERENT ELECTROLYTES
115
![Page 131: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/131.jpg)
»: .-•« m
116
LI
sm
1 0 1 0 1 0 10I < U A / C M •i ;i
Figure 32. Potentiodynamic test results of a-brass in 5 M NH4OH plus Cu(N03) 2solution.
![Page 132: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/132.jpg)
.r"™ISO
3 0 0
- 4 5 0 i i i I i ml i i i I i ml I i l l I m ],—1,7-1, Jj l.ljJ___1—LJ-LL11JI
10- 1
100
1 0 10 10 IC U A / C M A 2 i
1 0
J I 1 .J J X1.J4
1 0
Figure 33. Potentiodynamic test results of a-brass in 1 M NaNC>2 solution.
![Page 133: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/133.jpg)
M118
1 5 0
Ul 0
"1------ r ~l~ P 'TTTI--------- 1----- I— |—pTTTT]--------- 1---T T * f T 11 I I---------1----- 1 I | I I I I
/4 ?'/
-= = C ir'-“a..
X
I I i _ 1 j _ ui i i_L J .au
1 0
K U A / C M a Z)
Figure 34. Potentiodynamic test results of a-brass in 0.1 M CuS04 solution.
![Page 134: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/134.jpg)
VITA
Kun Lian w as born on February 11, 1957 in W uhan, Hubei province, People’s
Republic o f China. After completing his highschool education in 1975, he w ent to the
countryside where he did three years o f field work. In February, 1982, he received the
Bachelor o f Science D egree in the Departm ent o f Chemical Industry M achinery, at
South China Institute o f Technology, Guan-Zhoung, P. R. o f China. From February,
1982 to December, 1987, he w orked at W uhan Research Institute o f M aterials
Protection, M inistry o f M achinery Industry as associate corrosion engineer and
corrosion engineer. H e began his graduate studies at Louisiana State University in the
Interdepartm ental Program in M aterials Science in the College o f Engineering in Fall
1989, and received the M aster D egree in Engineering Science in August, 1991. After
receiving his M .S., he w orked at Louisiana State University School o f Dentistry,
Biomaterial Departm ent as a research associate, and at the same time he w as a part-
time student at Louisiana State University pursuing his Ph.D. in Engineering Science.
H e received his D octor o f Philosophy D egree at the Summer commencement, 1995.
119
![Page 135: A Study of the Stress Corrosion Crack Initiation Stage in](https://reader031.vdocuments.us/reader031/viewer/2022022004/621065106d6cb8532018c7d9/html5/thumbnails/135.jpg)
DOCTORAL EXAMINATION AND DISSERTATION REPORT
Candidate: Kun Lian
Major Field: Engineering Science
Title of Dissertation: a Study of the Stress Corrosion CrackInitiation Stage in Alpha-Brass
Approved:
P ' I 4 ; y >ior Professor and ChaiChairman
raduate School
EXAMINING COMMITTEE!
; t C ^ j u
Date of Examination:
0 6 / 1 9 / 1 9 9 5